There are two main factors that damage permanent ladle lining castables. First, excessive cracking occurs from repeated use. This is due to the castable’s inherent shrinkage or excessive water addition, which causes excessive linear shrinkage and, with repeated use, widens the cracks. During segmented casting, the castable fails to form a single piece at the joints, resulting in transverse cracks that widen during use. After repeated use, gaps develop in the asbestos sheet near the ladle shell, releasing stress in the permanent lining and causing cracks to widen. Second, insufficient castable strength during disassembly can lead to surface damage.
Comparative tests of low-cement, high-alumina permanent lining castables at different water addition levels revealed the following:
With increasing water addition, the apparent porosity of low-cement, high-alumina permanent lining castables increases, while the bulk density decreases. This, in turn, leads to a decrease in the castable’s compressive strength and flexural strength.
Multiple comparative tests have shown that increasing water addition significantly increases the linear shrinkage of the castable, which can exacerbate shrinkage cracks that occur during use. When the water content of low-cement castables increased by 2%, obvious shrinkage cracks appeared on the surface of the specimens. Furthermore, as the amount of water added increased, the castable was prone to particle segregation—a phenomenon in which particles sank and fines floated. Areas with more fines experienced increased shrinkage, leading to uneven internal stress and a greater tendency to crack.
Therefore, some simple methods for improving the performance of castables for the permanent lining of the ladle are as follows:
1. Controlling the amount of water added to the castable
The more water added, the lower the castable’s strength and density, the higher its apparent porosity and post-firing shrinkage. Therefore, while ensuring ease of construction and operability, water usage should be minimized to ensure optimal performance.
2. Effectively ensuring consistent construction timelines
Currently, permanent lining castables in steel mills are cast using bricks instead of molds, with intermittent, staged casting. Typically, the entire brick mold is constructed in three sections. Casting begins after the first section is completed, followed by the second section, and then casting continues, and so on. High summer temperatures or delays in casting for special reasons can easily cause the first section to initially set by the time the second section is cast. This can lead to poor connection between the two sections and horizontal delamination. This can also cause horizontal cracks at the joints after use. Therefore, proper connection should be ensured during construction to minimize the time between castings.
3. Establish a Reasonable Baking Schedule
Low-cement castables achieve their strength through hydration and cohesion. Baking requirements for low-cement castables are stringent, especially during the stage below 300°C where large amounts of physical and crystallized water are expelled. Improper baking can easily lead to flaking and cracking. A reasonable baking schedule must be established to ensure smooth water expulsion from the molded part. Depending on the construction thickness, natural curing should be performed for 16 to 24 hours after casting, followed by baking in the mold for approximately three days. After removing the brick mold and laying the working lining, baking should continue for at least 16 hours.
If a temperature control system is not available, adjust the gas flow to control the temperature. Baking is typically performed on low, medium, or high heat. The curing and baking time is adjusted based on the size of the ladle and the thickness of the permanent layer, generally ranging from 60 to 80 hours. The three baking times are usually 24h, 24~32h, and 12~16h respectively.
4. Optimizing the permanent lining castable formula
In order to solve the problem of excessive cracks, the castable formula was optimized and improved:
(1) A low-impurity expansion agent was added to the matrix to offset the partial shrinkage of the castable at high temperature. The castable with expansion agent improved the volume stability of the castable and improved the degree of crack expansion after repeated use of the castable.
(2) The upper limit of the castable aggregate particle size was increased from the original 8mm to 12mm. After testing, it was found that after the introduction of large particles, the amount of water added could be reduced by 0.5%, and the flexural strength at 1100℃ could be increased by 2MPa. This is because the presence of large particles not only plays a skeleton role, but also can change the direction of long cracks, help to prevent the expansion of cracks, and improve the volume stability of the castable.