The stopper rod is a kind of shaped refractory material used in the production process of the continuous casting machine. It can ensure the stability of the liquid level of the crystallizer, control the linear flow rate of molten steel, and ensure the surface quality and internal quality of the ingot. In actual production, the stopper plays a vital role in the stability of steelmaking production. Problems with the stopper , such as erosion, fracture, nodule, etc., will cause excessive fluctuations in the liquid level of the molten steel in the crystallizer. In severe cases, the continuous casting machine will be shut down prematurely or forced to be pulled down.
Analysis of the problem of stopper fracture
The slab continuous casting machine of a steel plant frequently has the problem of stopper fracture during the steel casting process, which seriously affects the normal production of the continuous casting machine. According to the statistics of the accident situation, the proportion of stopper head falling during the baking of the tundish or the pouring is 20%. The rest of the cases are that the stopper head falls during the pouring process or the stopper breaks at a position 650-700mm below the upper edge, and the fracture is “V” shaped, as shown in Figure 1. According to statistics, there were 12 rod stopper accidents in 2021, an average of once per month. Each accident caused unplanned shutdown of the continuous casting machine, requiring the tundish to be re-baked, the machine to be prepared, and casting to be started, disrupting the normal production plan. Therefore, it is urgent to solve the stopper problem, stabilize the production of the continuous casting machine, and reduce cost losses.

Figure 1 morphology of stopper rod fracture
Statistical classification of stopper accidents shows that the main factors affecting stopper fracture and stopper head falling are thermal shock, strength and stopper design and installation problems.
Thermal shock problem
Analyzing the material design of the stopper rod body and stopper rod head and the manufacturing process of the stopper rod, it is believed that the stopper material currently used meets the process requirements. The steel plant mainly uses carbon structural steel, high carbon steel and some medium carbon alloy steel, which has little erosion on the stopper. The stopper is not designed with slag line, and the scouring of the stopper head is not serious. Normal steel pouring for 15 hours, the stopper head has good flow control and uniform erosion. The material design is basically reasonable. From the fracture of the stopper head falling, the position is 50-60mm, and the fracture is flat. First of all, the problem of stopper manufacturing needs to be solved. The manufacturing process needs to be adjusted and strengthened. The uneven composition of the raw materials used to manufacture the stopper leads to stress, which is the direct cause of the stopper fracture.
The baking of the tundish on site is tracked, and the baking effect of the tundish is low. The tundish is baked with converter gas, the calorific value is generally 1300×4.1868kJ/m³, the baking time is 3h, the stopper is in an open state during the tundish baking, the baking temperature is 1000℃, the tundish is baked without sealing, and the flame overflows seriously during baking. Poor baking effect of the stopper will lead to uneven thermal stress of the stopper refractory material, thus generating microcracks. During the casting process, the stopper works in an extreme environment, and any small defects will be magnified.
Strength problem
The problem of stopper slag line fracture generally occurs 1~2 furnaces after the steel casting nozzle is replaced, after the bonding is restored, and during the tundish quick change process. Analysis shows that when the stopper is closed during the steel casting process, it is subjected to lateral and longitudinal forces to crack and then break.
The strength of the stopper body is analyzed, and it is believed that the strength of the stopper is low in the hot state, and it is easy to break under the condition of molten steel flushing or stress, and the strength of the stopper rod body needs to be strengthened.
Design and installation of stopper rod
The installation of stopper rods on site was tracked and analyzed as follows: ① There are problems with the stopper rod design. When the stopper is opened during steel pouring, the stopper rod is 200mm higher than the tundish cover. According to the normal design, the stopper rod is 50mm higher than the tundish cover to meet the requirements. The stopper is too long. When the stopper rod is closed in an emergency, it is subjected to huge external force and is prone to breakage. In particular, the slag line is the position where the stopper rod changes diameter, and this part is weaker; ② There are problems with the installation of the stopper rod. The main reason is that the stopper rod is installed offline, and there may be shaking damage during the process of putting the tundish online. The installation of the stopper rod requires a “gnawing head”. The existence of the “gnawing head” causes lateral force when the stopper rod is closed, causing cracks in the stopper rod head or the weaker part of the stopper rod. When the stopper rod is closed during the steel pouring process, the operator changes the mode from automatic to manual, and then presses the gate handle hard to close the stopper rod, which also aggravates the damage to the stopper rod.
Improvement measures
Improvement of stopper rod fracture problem
In view of the above problems, the current stopper rods are considered to be improved. The specific solutions are as follows:
(1) Under the premise of meeting production requirements, the material is fine-tuned to appropriately improve the thermal shock resistance of the stopper rod and strengthen the neck strength of the stopper rod. The adjustment idea is: introduce SiC powder into the production ingredients of the tundish stopper rod, focusing on the stopper head and slag line position, and design a composite structure for the stopper rod to improve the comprehensive mechanical properties of the stopper rod and reduce the linear expansion coefficient. When 5% SiC powder is added, the room temperature and high temperature flexural strength of the magnesium carbon rod head material are 8.2MPa and 9.4MPa respectively, and the average linear expansion coefficient is 7.1×10-6/℃. No obvious cracks are observed after 3 thermal shock cycles at 1100℃.
(2) Adjustment of stopper length. The stopper currently in use is too long, reaching 1750mm, which increases the difficulty of stopper rod production. It will also amplify the lateral force generated by the flow of molten steel during use, causing the rod body to break after being stressed. Based on the site, the stopper rod length is adjusted to 1650mm.
(3) Optimize the stopper rod head, change the shape of the stopper head from spherical to conical, improve the flow control accuracy of the stopper, and change the size of the stopper head from 60mm to 45mm.
Improvement of stopper rod installation method
Currently, the stopper rod is installed in the repair area, and the vibration during the transportation of the tundish will have an adverse effect on the stopper. Improve the existing stopper installation process, change from offline installation to online installation before the tundish is baked, and reduce the impact of the tundish transportation process; in addition, before debugging the stopper, check whether the shutter beam is deformed, observe whether the stopper is straight, cancel the “head biting” during installation and debugging, strictly align, and avoid the stopper from being broken due to the lateral force when the stopper controls the flow.
Optimization of stopper rod baking system
Optimize the stopper baking system for thermal shock problems. When the tundish is covered offline, the edge of the tundish is sealed, and it is strictly sealed before baking to improve the baking effect of the tundish; when the tundish starts to be baked, the stopper is in a closed state. After the tundish is baked for half an hour, the stopper is opened, which is conducive to the baking of the stopper and the upper water inlet. Revise the tundish baking system and stipulate a reasonable baking time. Long-term baking shortens the life of the tundish and even wastes the tundish. The fire cannot be stopped during the baking process, otherwise the tundish will be disposed of as a waste; strictly control the opening of the gas valve according to the tundish baking curve to ensure that the temperature rises to above 1000℃ during the baking period of 1~2h.
Improve the stopper rod operation during the pouring and steel pouring process
For the existing habit of “watching the rod” during the tundish baking process, it is changed to “watching the rod” by stopping baking before pouring. If there is a small deviation in the stopper, fine-tune the stopper to reduce the negative impact caused by stopping baking and vigorously adjusting the stopper rod during baking.
During the process of changing the nozzle, recovering the adhesion, and changing the tundish during steel pouring, the mode is first changed from “automatic” to “manual”, the operator holds the stopper handle, the stopper is closed by its own gravity, and then the operator presses the handle to close the stopper and perform subsequent operations.
Implementation process and effect
According to the above measures, it is implemented in two steps: first, the tundish baking system is improved, the tundish sealing is strengthened, the stopper baking effect is improved, and the stopper rod installation and use operation are improved; secondly, the stopper is optimized, the manufacturer designs the stopper improvement drawings, and the mold and stopper are made, and the conditions are met for on-site testing.
The improved stopper is tested on-site, and the stopper baking, pouring and steel pouring processes are tracked. It is required to lift the stopper out every time the machine is stopped. The casting steel types include Q235, Q345, 45#, 50# and other steel types. The condition of the stopper head is observed, the flow control is good, and the stopper head is uniform.
The implementation of the above measures has achieved certain results. The continuous casting machine shutdown accidents caused by stopper breakage have gradually decreased. In 2022, the steel plant had only two stopper rod breakage accidents, which was 10 times lower than in 2021, and the use of stopper rods has become stable.
Conclusion
By controlling the trace additives added during the stopper production process and optimizing the stopper shape, the thermal stability and flow control accuracy of the stopper can be improved, which is conducive to stabilizing the crystallizer liquid level, reducing the number of stopper switches, and improving the use effect of the stopper.
Through the improvement and optimization of on-site stopper installation, baking and use, the problem of stopper breakage caused by thermal shock and mechanical damage is reduced, and the use of tundish stopper is stabilized.
FAQ
What are the differences in fracture morphology between “thermal shock fracture” and “mechanical fracture” of stopper rods? How can they be quickly determined?
Answer: Thermal shock fracture usually occurs due to insufficient preheating or the initial stage of casting. The fracture surface is smooth and mostly occurs on the upper part of the rod. Mechanical fracture (such as uneven stress on the mechanism) often shows obvious stress tear marks or oblique cracks. By observing whether the fracture surface is accompanied by severe chemical corrosion, it is possible to distinguish between material problems and operational errors.
In pursuing “long-life” continuous casting, how to balance the corrosion resistance and thermal shock resistance of stopper rods?
Answer: This is a balance point in material design. Increasing the carbon content can improve thermal shock resistance, but it will reduce corrosion resistance. The current industry trend is to adopt a composite structure design: using high-zirconium carbon material for corrosion resistance in the slag line zone, while using high-alumina carbon material inside the rod to ensure toughness, and combining micronization technology to optimize the matrix structure.