lmm@magnesiacarbonbricklmm.com

Technical support and construction service team

Analysis and preventive research on the causes of graphite electrode breakage in ladle refining furnaces

Based on the production practice of the ladle refining furnace of the Tianjin Iron Works Co., Ltd. steelmaking plant, this article analyzes the reasons for electrode breakage during the ladle refining process and puts forward relevant technical points to provide a reference for achieving safe production and energy saving and consumption reduction.

Keywords: iron and steel metallurgy; LF ladle refining; graphite electrode; energy saving and consumption reduction

1 Introduction

In the production of ladle refining furnace, thermal compensation is achieved by heating the molten steel through graphite electrodes. The consumption of graphite electrodes accounts for 15%-20% of the total production cost. Due to fluctuations in the electrode price market, when its price rises, this consumption proportion further increases. The consumption of graphite electrodes includes burning and peeling under normal conditions, as well as abnormal electrode breakage. Once an electrode breaks, one or even several electrodes will be directly scrapped, resulting in huge losses. At the same time, when the electrode breaks, it is very difficult to handle, resulting in increased labor intensity and even production interruption. What’s more, improper handling may cause casualties. It can be seen that electrode breakage is extremely harmful, and efforts must be made to reduce and avoid such accidents.

2 Reasons for graphite electrode breakage

The breakage of graphite electrode in the production of ladle refining furnaces is mainly caused by the breakage of weak points such as electrode joints under the action of various mechanical forces.

2.1 Causes of graphite electrode weakness

The fundamental reason for the electrode to break is that there is a weak spot in the electrode. Each phase electrode is composed of 2 to 3 sections connected by threads. Due to the discontinuity of the material, the flexural strength of the joint is less than that of other parts, thus forming a weak point. Due to damage caused by collisions during transportation, installation, use, etc., electrodes often have visible or invisible cracks and other defects before installation, further reducing the strength of the electrode joint and increasing the possibility of breakage during production. As shown in Figure 1, the electrodes are improperly installed, there are debris at the interface, and the joints are not aligned or tightened, resulting in gaps at the connections, resulting in a large contact resistance between the connected electrodes. Due to the huge current during smelting, the electrodes The contact between the joint and the two connected electrodes generates high temperature and causes ablation; or the flame generated during smelting enters the gap, causing further erosion of the peripheral parts of the gap, further reducing the strength of the already weak joint.

graphite electrode

Figure 1 Ablation of electrode interface with gaps during smelting

2.2 Analysis of mechanical forces acting on graphite electrode

2.2.1 Electric forces generated during smelting

There are huge currents of tens of thousands of amperes in the electrode system during smelting in the ladle refining furnace. As shown in Figure 2, due to the electromagnetic induction, a strong electric force is generated between the electrode and the conductive cross arm. The direction of this force is away from the polar center circle and points to the furnace wall. The outer electrodes (phase A and phase C) have a tendency to move outward; the middle phase (phase B) electrode has a tendency to move downward. This movement of the electrode, coupled with the uneven distribution of the charge on the molten steel surface, and even due to the crusting of the slag surface, the electrode is directly inserted into the molten steel, causing the voltage and current on the electrode to fluctuate greatly, and then the electric force continues to change. This cyclic action eventually causes the entire electrode system to vibrate violently. If the mechanical vibration frequency of the electrode cross arm is close to or synchronized with the electromagnetic force vibration frequency, the electrode will resonate, causing the vibration of the entire system to be greatly aggravated, causing the electrode joint to repeatedly bend slightly, resulting in fatigue fracture of the electrode. The electric force vibration generated by the electrode system is often further aggravated by superposition with the automatic adjustment movement of the electrode. The electrode adjustment system uses a computer to analyze the voltage and current on the electrode system to keep the arc heating current close to the set current point to achieve the purpose of controlling the heating speed. The violent fluctuations in voltage and current cause the electrode to move up and down continuously, eventually causing strong vibrations in the entire system.

Figure 2 Electrodynamic forces on electrodes during smelting

2.2.2 Influence of slag layer during smelting

The distribution of slag layer on the surface of molten steel has a crucial influence on the electrodynamic forces mentioned above. When the slag layer is fully melted, the viscosity is moderate, and it has a certain foaming effect, the arc submergence effect is good, the current and voltage are relatively stable, the electrode is almost not adjusted up and down, and the whole system runs very stably. When the viscosity of the top slag is too high, the slag surface fluctuates under the stirring of the bottom argon gas. Due to the high viscosity of the top slag, it is difficult to flow and deform, and it cannot be reset in time. The electrode head is easy to leave the slag layer or contact with the molten steel, and it cannot fully submerge the arc. When the viscosity of the top slag is too low, the slag surface fluctuates too actively and cannot fully submerge the arc. At the same time, the top slag with too low viscosity is generally more difficult to have sufficient foaming properties, the slag layer is thin, and the submerged arc effect is insufficient. Usually, after the steel is tapped from the converter, lime, fluorite and other slag materials are added to the surface of the molten steel. After the tumbling action of the bottom-blown high-pressure argon gas, these materials are often still not evenly distributed on the surface of the molten steel, and sometimes even piled up on the surface of the molten steel. Due to cost constraints, the slag materials used as refining furnaces are generally simple materials, and the more expensive calcium aluminate synthetic slag is rarely used. For example, the main component of lime blocks is CaO, which has a high melting point and cannot be melted at the temperature of molten steel (1500-1600℃). Therefore, in the furnace without hot slag top addition, a hard slag shell is often formed on the surface of the molten steel. The conductivity of this slag shell is very different from that of the molten steel, and it also hinders the normal automatic adjustment movement of the electrode. When the electrode is inserted into the slag shell but cannot be completely broken, the violent vibration generated by the electrode system can directly break the electrode whose head is fixed by the slag shell.

2.2.3 Other mechanical external forces

During production, due to various reasons, graphite electrodes are often broken due to the impact and collision of various external forces. Because the ladle used for refining is stained with slag, steel and other debris along one side, the furnace cover tilts to one side after it is lowered. At this time, when the electrode is lowered for smelting, the electrode will be broken by the tilted furnace cover. This situation is relatively common and often causes the three-phase electrodes to break at the same time. Special attention must be paid. The electrode, conductive cross arm, and furnace cover system are deformed, stuck or loose, which may break the electrode when the electrode is lowered. During the sliding electrode process, the suspended electrode is not accurately aligned, and the electrode may also be broken when the clamp is clamped. If the sliding electrode is too long, the electrode will be hit by the ladle when it is turned back to the turntable.

3 Preventive measures for graphite electrode breakage

Through the analysis of the causes of electrode breakage in the production process of the ladle refining furnace and combined with production practice, the following preventive measures are proposed in three aspects: protection before electrode installation, correct installation of electrodes, and operation methods during smelting.

3.1 Protection before graphite electrode installation

Before installing the electrode, protect it well to avoid collision. Before lifting, carefully confirm that the lifting device is reliable and the connection is firm. During the lifting process, ensure that the overhead crane moves steadily and slowly, and the electrode joint protective cover should be retained before screwing.

3.2 Correct installation of graphite electrode

Before installing the electrode, the electrode interface should be carefully purged to ensure that there is no debris at the interface. If the thread is wrongly screwed during screwing, it should be reinstalled and should not be tightened forcefully. There should be no gap at the electrode interface after installation. A spring buffer device can be installed on the electrode hanger, as shown in Figure 3, to ensure the protection of the electrode when the overhead crane is not properly matched. Due to various reasons, electrodes from different manufacturers may be used at the same time in actual production. During the installation of the electrode, it should be ensured that the electrodes used in one item are products of the same manufacturer and model as much as possible to avoid problems such as inconsistent thermal expansion rate, strength, density, size, or poor interface matching between electrodes with different performances, which increases the risk of breakage at the electrode interface.

Figure 3 Electrode hanger with spring buffer device

3.3 Operation method in smelting

3.3.1 Treatment measures for top slag crust

After the molten steel arrives at the station and is connected to the argon pipe, high-pressure bottom blowing should be turned on to break the slag crust on the molten steel surface and promote the unmelted furnace charge to be distributed as evenly as possible. For example, the slag surface is crusted due to the long waiting time before refining, and even a small amount of molten steel overflows from the slag shell to form a steel shell. To address this problem, a certain amount of slag such as lime and fluorite can be added to form a relatively uniform and loose slag layer on the molten steel surface, which plays a buffering role before the slag shell melts to prevent the electrode from being subjected to excessive external force impact; if there is a steel shell on the slag surface, it must be covered with slag, and blind electrode operation is prohibited.

3.3.2 Stable arcing operation

When starting smelting, a relatively small current and voltage should be used to start the arc smoothly. When the charge is initially melted and a certain arc submergence effect is achieved, the current should be increased to a normal level first, and short arc heating should be used to accelerate electrode ablation and produce a certain amount of CO gas to help arc submergence. When the arc submergence is stable, the voltage can be increased and the current can be reduced to use long arc heating to reduce electrode consumption and carbon increase in molten steel.

3.3.3 Strengthening bottom blowing of argon and process slag condition control

Stirring molten steel and top slag through bottom blowing of argon is one of the basic functions of the ladle refining furnace. A large amount of argon can achieve full contact between steel and slag, use the physical heat of molten steel to help slag melting, and quickly mix various molten slag materials, thereby increasing the slag melting speed. However, an excessive amount of argon causes the steel and slag in direct contact with the electrode to have excessive kinetic energy, directly impacting the electrode; and causes violent fluctuations in the slag surface, arc exposure, and frequent and large-scale movements of electrode lifting and lowering, thereby increasing the risk of electrode breakage. In actual production, the slag condition in the furnace can be understood by manual or automatic analysis of the smelting noise and the amplitude and frequency of electrode rise and fall. The manual analysis method is that the noise is loud, crisp and bright, indicating that the arc submergence effect is poor. It may be that the slag layer is too thin, the slag fluidity is too strong, and the argon gas blowing from the bottom is too large. The heating gap should be used to confirm as soon as possible, find out the specific cause, and take corresponding measures. The noise is generally too dull, accompanied by periodic large noise, indicating that the slag is too sticky. The overall arc submergence is good, but when the Co produced by smelting and the bottom blowing argon gas accumulate to a certain amount, they break through the slag layer in a concentrated manner, resulting in periodic and temporary arc exposure. When the noise is relatively dull and remains stable for a long time, it indicates that the slag condition and bottom blowing are relatively reasonable.

3.3.4 Avoid and reduce external forces

During smelting, large pieces of materials that exceed the specification shall not be put into the furnace to prevent the electrode from colliding with large pieces of materials and breaking when the electrode is lowered. Pay special attention to the steel and slag sticking on the edge of the ladle. It should be specially confirmed after each ladle placement. When it is found that the edge of the ladle used is stained with a lot of debris, special attention should be paid. If the furnace cover is tilted after lowering, the furnace cover can be slightly lifted to ensure that the furnace cover is flat, and the relevant personnel should be notified in time to handle the ladle. Check various mechanical and electrical devices of the electrode system frequently. Pay attention to the electrode, conductive cross arm, and furnace cover system during smelting. If deformation, jamming or loosening is found, repair it in time. During the sliding of the electrode, the overhead crane must be accurately directed to ensure that the electrode can be tightened only after accurate centering. After sliding the electrode, it must be carefully confirmed. If the electrode is found to be too long, it must be handled in time.

4 Conclusion

The main reason for the breakage of graphite electrode in the production of ladle refining furnaces is the action of various internal and external mechanical forces. By doing a good job of protecting the electrode before installation, installing it correctly, optimizing the smelting operation, especially stabilizing the arcing and slag-melting conditions in the early stage of smelting, ensuring that the slag condition and bottom blowing argon control meet the refining requirements, and timely maintaining equipment, etc., the electrode breakage accident can be prevented.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information