During the continuous casting process, tundish nozzle blockage has occurred many times, which has reduced the casting speed and even interrupted the injection flow. The sticky slag in the tundish nozzle can also cause the submerged nozzle to deviate, causing slag wrapping and cracks, which has a certain impact on normal production. According to statistics, the number of unplanned shutdowns of tundishes due to nozzle blockage accounts for about 3.7%. Domestic and foreign experts have conducted a lot of research on the problem of tundish nozzle blockage. Drawing on their experience, we have conducted a long-term tracking analysis of the continuous casting production of our department.
In the process of continuous casting, the role of the submerged nozzle is to control the amount of molten steel injected from the tundish into the crystallizer and the flow of molten steel in the crystallizer. It plays a very important role in stabilizing operation and ensuring the quality of molten steel. When alumina adheres to the inner wall of the submerged nozzle, the nozzle casting flow will deviate and the molten steel surface will fluctuate in the crystallizer, which will not only deteriorate the quality of the continuous casting billet, but also seriously affect the realization of multi-furnace continuous casting.
Cause Analysis
There are two main phenomena of tundish nozzle blockage. One phenomenon is the low-temperature flocculation of molten steel caused by various reasons. The outer circle of the adhesive in the water outlet is dark gray, while the inner circle is a small amount of white objects. After sampling, the components are analyzed as shown in component (1) in Table 1, and the main components are Fe and FeO. Another phenomenon is that the sediment attached to the inner wall of the water outlet of the tundish accumulates more and more, causing the inner diameter of the water outlet to narrow or even block the water outlet. The adhesive in the water outlet is a white object. After sampling, the components are analyzed as shown in component (2) in Table 1, and the main component is Al₂O₃.
01 Reasons for the main components of Fe and FeO in the blockage
(1) Insufficient baking of the water outlet of the tundish
Due to insufficient or unstable coal gas, abnormal production, frequent continuous casting and ladle replacement, the use of the tundish is tight, and the tundish is hastily used if the baking does not meet the requirements; after the molten steel is injected, the temperature of the water outlet is low and cold steel is easily formed, which makes the inner diameter of the water outlet smaller or blocked.
(2) Excessive cooling of the tundish steel liquid
During the continuous casting process, if the molten steel temperature is too high or there is a concern about steel leakage at high casting speeds, scrap steel is often added to the tundish steel liquid for cooling. Since each type of steel has its own liquidus temperature, once the temperature is excessively cooled, the molten steel temperature approaches or reaches its liquidus temperature, and the molten steel will solidify or freeze. Statistical data show that when the superheat △T is less than 5℃, the probability of flocculent flow is 100%; when the superheat △T is between 6-10℃, the probability of flocculent flow is 31%.
3) The molten steel temperature does not meet the standard
The molten steel temperature itself does not meet the standard, which is also a factor that cannot be ignored in causing low-temperature dead flow. This phenomenon occurs in the following situations: (1) When the metering of the converter unloading system is inaccurate, the molten steel temperature is too high, and steel is directly tapped after adding. (2) Before the new ladle is used, the baking temperature does not reach above 800℃, and the molten steel temperature drops too much after tapping. (3) There were large pieces of steel at the bottom of the accident ladle that were not cleaned up, and the furnace was not notified in time. (4) During the steel tapping process, slag fell into the ladle at the furnace mouth.
02 The reason why the blockage is mainly composed of Al₂O₃
Due to the use of aluminum blocks for deoxidation during the smelting of SPHC, and deep deoxidation. The deoxidation product is mainly Al₂O₃. It was observed that the inner wall of the nozzle was adhered to floccules in two colors, dark yellow and blue; the same substance was also adhered to the surface of the corresponding part of the nodule cold steel.
The flocculent nozzle was scanned by an electron microscope and analyzed. It was found that although the inner wall adhesives of the two nozzle samples had different appearance colors, they had similar chemical compositions. They were all oxides mainly composed of Al₂O₃, and contained a small amount of CaO, SiO₂ and MnO. The appearance and morphology show that the blue adhesive is denser, the yellow adhesive is slightly looser, and the analysis of the adhesive on the surface of the nodule cold steel shows that its chemical composition is the same as that of the nozzle adhesive, which is mainly composed of Al₂O₃ oxides and contains a small amount of oxides. The cross-section analysis of the cold steel found that the sample contains a large number of dispersed inclusions. The inclusions are generally divided into two categories, one is MnS inclusions, and the other is Al₂O₃-rich CaO, SiO₂ and MnO, TiO₂ composite inclusions. The second type of inclusions is irregular or nearly spherical in shape, with a size of about 10 microns and small particles.
The typical inclusion morphology is: Al₂O₃ particles inside, and more SiO₂, MnO, and CaO components in the outer layer, indicating that these inclusions are likely to come from aluminum deoxidation products that have not floated. In molten steel with high oxidizability, Si and Mn deoxidation or secondary oxidation products form composite inclusions with Al2O2 as the core. These inclusions are solid at the continuous casting temperature and continuously adhere and accumulate on the inner wall of the tundish nozzle. The calcium treatment does not convert Al2O2 into liquid calcium aluminate, and the treatment effect is poor, which eventually causes nozzle nodules.
Measures taken
01 Low-temperature flocculent flow caused by temperature
The following measures were mainly taken:
(1) Regularly check the gas baking pipeline of the tundish to prevent the occurrence of gas pipeline blockage or gas leakage, ensure sufficient baking gas, and strictly implement the principle of “low fire first, medium fire, and high fire” when baking the tundish to ensure that the temperature of the tundish reaches above 1000℃ when in use. In addition, in addition to meeting normal production, the knotting of the tundish must also ensure a certain margin in case of emergency.
(2) Improve the temperature and component compliance rate of the molten steel at the end of blowing to ensure that the temperature of the continuous casting molten steel is appropriate and the composition is qualified; when continuous casting starts, if the temperature of the molten steel in the tundish is low, the pouring time should be postponed to increase the temperature and static pressure of the molten steel in the tundish when pouring, prolong the floating time of inclusions, and improve the success rate of pouring.
(3) In order to prevent excessive cooling of the tundish steel liquid during pouring, the contractor is required to measure the temperature of each furnace of steel at least three times. In addition, the appropriate pouring temperature of carbon structural steel and low-alloy steel is determined according to the chemical composition of each steel grade to ensure that the superheat of the molten steel is within the range of 10~20℃, and the contractor is urged to strictly implement it.
02 Low-temperature flocculence caused by Al₂O₃
By adding a certain amount of calcium to the molten steel, the high-melting point Al₂O₃ combines with CaO to form low-melting point calcium aluminate, which is easy to diffuse and float. To reduce the formation of manganese sulfide inclusions, the method of calcium treatment of molten steel is usually adopted. To achieve successful calcium treatment, attention must be paid to the amount of calcium added. If the calcium treatment is not properly controlled, it will not only fail to achieve the expected metallurgical effect, but will also deteriorate the pouring performance of the steel.
There are two reasons for the blockage of the water nozzle of calcium-treated molten steel: one is that the amount of calcium added is not enough, and Al₂O₃ cannot be converted into 12CaO₇Al₂O₃, forming CaO₆Al₂O₃, CaO₂Al₂O₃, CaOAl₂O₃, and CaO3Al₂O₃; the other is that the amount of calcium added is too much, and calcium will combine with S in the steel to form CaS (melting point 2500℃). In the process of adding calcium to the molten steel, as the calcium content in the molten steel continues to increase, the calcium content in the inclusions also increases, forming complex inclusions, among which CaO₆Al₂O₃ and CaO₂Al₂O₃ have melting points above 1700℃, which must be avoided in actual production. Therefore, calcium treatment must ensure that enough calcium is added to the steel, and the appropriate wire feeding amount should be controlled at 1.5-2.5 meters/ton. At the same time, the refined slag should also be added appropriately to make it have sufficient ability to absorb inclusions.
At the same time, the sulfur content in the molten steel is controlled, and the sulfur and acid-soluble aluminum content in the molten steel are coordinated. In order to reduce the probability of CaS generation during calcium treatment of molten steel, the sulfur content of the molten steel is required to be low, and the sulfur content of the incoming molten steel must be controlled. Achieve the coordination of molten steel [Als], S, and Ca to ensure that the molten steel is denatured after calcium treatment of the molten steel, reduce the total oxygen content, and improve the purity of the molten steel. After optimizing the process, the flocculent flow phenomenon of the continuous casting nozzle has been basically solved, and the Al₂O₃ inclusions larger than 30 microns have been basically removed, stabilizing the production of the continuous casting machine. Calcium treatment of low-carbon aluminum deoxidized molten steel can transform Al₂O₃ inclusions into low-melting point inclusions, which can significantly improve the castability of the molten steel and prevent nozzle adhesion and blockage.
Conclusion
(1) The main components of the blockage are Fe and FeO. The main reason is that the tundish water inlet is not baked enough, the tundish steel liquid is cooled too much, and the molten steel temperature is not up to standard, which can cause low-temperature flocculent flow. It can be completely avoided through improvement measures.
(2) The main component of the blockage is A1203 because the aluminum deoxidation product A1203 is not discharged in time and the calcium treatment is not appropriate.
(3) In order to reduce the probability of CaS generation during calcium treatment of molten steel, the sulfur content of molten steel must be low, and the sulfur content of the incoming molten steel must be controlled. Achieve the coordination of molten steel [Als], S, and Ca.