Analysis of causes and countermeasures for the peeling of the lining of the medium frequency induction furnace

In industrial furnaces, especially kilns using amorphous refractory materials as linings, lining peeling is one of the key factors that cause the kiln to shut down and shorten its service life. Taking the medium frequency induction furnace as an example, the causes and countermeasures of the peeling of the induction furnace lining are analyzed in detail.

Peeling phenomenon of induction furnace lining

20 tons of medium frequency induction furnace, lining material MS1001a, 0.8% B2O3 addition, after the lining was used for 4 furnaces, when the lining was checked, it was found that the surface materials of the sintering layer of the side wall and the bottom of the lining fell from the surface of the lining in the form of blocks or pieces, and then pits appeared on the surface of the sintering layer of the lining.

Peeling of lining caused by water vapor

At 100℃ and a standard atmospheric pressure, the specific volume of water is: 0.00104344m3/kg (liquid), 1.6736m3/kg (steam). Therefore, the volume expands 1618 times after water turns into water vapor.

If the moisture content of the lining material is too high or damp, and the prefabricated parts and coil slurry are newly replaced and not completely baked to drain the moisture, when the lining is knotted and sintered, the rapid temperature rise will cause the large amount of water vapor generated inside the lining to be unable to be quickly discharged and pressurized, and finally break through the surface of the sintered layer of the lining, causing the surface of the sintered layer of the lining to be pushed out and peel off, and the above situation will occur.

Spalling of the induction furnace lining caused by mechanical damage

In the early stage of the first furnace sintering, the sintered layer of the lining has not yet established a strong strength and is not thick enough. If a large piece of furnace charge is added to the furnace, it will cause the lining to be “forced” to peel off.

Spalling of lining caused by different expansion coefficients

This phenomenon often occurs at the junction of the hot surface of the lining that is wetted by molten iron and non-wetted. The interface between the wetted hot lining and the non-wetted cold lining will separate due to the different expansion coefficients during the change of hot and cold cycles.

Spalling of induction furnace lining caused by rapid hot and cold changes

Rapid hot and cold temperature changes exceed the lining’s thermal shock resistance and crack healing capabilities.

Spalling of lining caused by stress

This situation usually occurs at the bottom of the furnace. In the middle and late stages of the lining’s life, the lining is eroded around and the bottom of the furnace is uneven. When the lining is heated, the expansion stress will cause the lining to burst and spall.

induction furnace

Countermeasures for spalling defects of the induction furnace lining

The spalling of the lining is mainly caused by water vapor and stress, and others are supplementary.

Therefore, for moisture, the newly repaired coil glue and the replaced prefabricated parts before knotting the lining can be heated by electric furnace after setting up the crucible mold in the furnace and baked at high temperature to completely exhaust the crystal water and water vapor in them; the purchased furnace lining materials should be used as soon as possible and moisture-proof measures should be taken to prevent the lining from getting wet again; the coil should be tested for water and pressure before building the furnace to prevent micro-leakage of the internal circulating water, which will cause moisture to enter the lining. The temperature should be raised slowly during the sintering operation, and the crucible mold should have exhaust holes to ensure the normal overflow of moisture.

For other types, small and light pig iron should be used when adding materials to the cold furnace, and large pieces should not be used to violently impact the cold lining; at the same time, the appropriate furnace lining material knotting method and baking process should be selected, and the furnace bottom must be leveled before the crucible mold is placed to prevent stress peeling.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information