Analysis of Causes and Improvement Measures for Damage to Permeable Brick in Steel Ladles

The refining ladles in steel rolling mills use integral Permeable Brick. During use, issues such as spalling, steel trapping in narrow slits, and inability to be blown open occur. Measurements show that the length of the remaining brick core is approximately 180mm, and the monthly permeability is 99.2%. By analyzing the causes of permeable brick damage, corresponding measures were formulated to increase the core length and improve permeability.

01 Analysis of Causes of Permeable Brick Damage

1.1 Core Delamination of Permeable Bricks

After hot repairs, the ladle temperature is approximately 900℃ when it is placed in the converter. The converter’s final temperature is approximately 1630℃. The rapid heating and cooling caused by this temperature difference leads to core delamination of the permeable bricks, typically 10-20mm thick. Furthermore, because the tapered delamination portion does not fall off after core delamination, it affects the permeability of the molten steel in the ladle.

1.2 Fracture of the Aerated Brick Seat Brick

Rapid cooling and heating due to temperature differences can also cause fractures in the aerated brick seat brick, with fracture heights ranging from 100 to 200 mm. The brick core, lacking the protection of the seat brick, will also fracture due to erosion from the molten steel. Such fractures are extremely dangerous, especially in the later stages of the aerated brick’s service life, as the remaining brick is shorter, easily leading to steel leakage at the bottom of the ladle.

1.3 Low Strength and Poor Erosion Resistance

When cleaning the aerated brick with an oxygen lance during hot repairs, the normal cleaning rate is 9-12 mm/furnace. If the strength is insufficient, the brick core height decreases significantly with each cleaning, causing the aerated brick to be used before its specified normal lifespan, affecting the normal turnover of the ladle and causing production instability.

1.4 Erosion and Damage from Molten Steel

When inert gas is sprayed through the aerated brick, the airflow impacts the exposed aerated brick, creating a certain impact force. The high-speed flowing molten steel and airflow interact to form a vortex. When the aerated brick is higher than the seat brick, its protruding parts are eroded and sheared by the vortex, forming annular grooves.

1.5 Excessive Oxygen Burning Damage

If the ladle is not refilled promptly after continuous casting, cold steel will form at the bottom of the ladle. This requires cleaning the core of the permeable bricks using an oxygen lance. However, this direct oxygen burning causes rapid damage to the permeable brick core.

1.6 Misaligned Permeable Brick Core

When cleaning the permeable bricks, the oxygen lance is used to press against the core. This concentrates the oxygen in one point, easily causing misalignment of the core. The core surface becomes sloping instead of flat, with a height difference exceeding 50mm. Misalignment results in poor permeability, and each cleaning session exacerbates the misalignment, leading to premature removal from the production line.

1.7 Low Backflushing Gas Pressure

The backflushing gas is nitrogen at 0.5MPa, while the oxygen lance pressure is 0.8MPa. During oxygen cleaning, molten steel is blown into the narrow gaps of the permeable bricks. Upon cooling, this blocks the gaps, causing poor permeability. Subsequent hot cleaning will further exacerbate the damage to the permeable brick core.

1.8 Detachment of Corundum Material and Bottom Bricks Around Permeable Bricks

During bottom bricklaying, a 50-100mm wide layer of self-flowing corundum material is poured around the permeable brick base to protect it. Due to insufficient strength of the self-flowing corundum material or construction problems, the corundum material around the permeable brick base detaches, allowing molten steel to seep in and causing the permeable brick base to crack; alternatively, the bottom bricks around the permeable brick base may crack, allowing molten steel to seep in and causing both the surrounding corundum material and the permeable brick base to crack.

02 Measures to Improve the Quality of Permeable Bricks

2.1 Improving the Peeling Resistance of Permeable Bricks by Adding Zirconium-Based Materials and Tabular Corundum

Adding pre-synthesized zirconium-based materials to permeable bricks can modify alumina-chromium permeable bricks. The toughening effect of ZrO2 can significantly improve the thermal shock resistance of permeable bricks. Tabular corundum has high strength, giving permeable bricks excellent thermal volume stability and good thermal shock resistance.

2.2 Improving the Erosion Resistance and Strength of Permeable Bricks

To improve the high-temperature resistance of permeable bricks, it is necessary to minimize the impurity content in the raw materials. Adding α-Al2O3 micro powder and controlling the addition of spinel particles (1-0 mm) at 16%-20% can improve the strength of permeable bricks and enhance their resistance to oxygen purging.

03 Standardized On-site Operation

3.1 Timely Refilling of Pouring Residue

If the pouring residue is not promptly refilled after continuous casting, cold steel will form on the bottom of the ladle, and slag will also form a crust, making it difficult to clean the permeable bricks and affecting their permeability. Prolonged oxygen-fired cleaning will also accelerate the damage of the permeable bricks. Therefore, the time from the completion of continuous casting to the refilling residue must be specified. On-site statistics show that the residue will not solidify within 10 minutes, but this is also related to the refining station temperature, steel grade, and ladle condition.

3.2 Strictly Prohibit Operation with Oxygen Lance Pressing Against Permeable Bricks

When cleaning permeable bricks with an oxygen lance, the oxygen tube must not be pressed against the brick core to burn oxygen. This will accelerate the damage of the permeable bricks and easily lead to uneven burning. Therefore, the tip of the oxygen lance should be a certain distance from the brick core, usually around 50mm.

3.3 Installing a Flow Meter

Another factor contributing to excessive oxygen-fired cleaning of permeable bricks is the operator’s judgment based on experience. The blackening of the permeable brick core accompanied by gas noise indicates good permeability. To prevent excessive burn-off and address the issue of relying on experience for operation, a flow meter was installed at the ladle hot repair station, with a set alarm threshold. The alarm threshold indicates that the permeability of the permeable bricks meets the requirements for refining argon blowing, and an audible and visual alarm is used. This allows operators to stop operation once the permeable bricks reach the flow alarm threshold, reducing human-induced burn-off and avoiding biases caused by human judgment of permeability.

3.4 Increasing Backflushing Gas Pressure

The low-pressure nitrogen backflushing gas was replaced with high-pressure nitrogen, increasing the pressure from 0.5 MPa to 1.2 MPa, preventing molten steel from entering the narrow gaps. Simultaneously, the backflushing time was adjusted; instead of starting backflushing at the ladle turning machine, it was changed to starting just before cleaning the permeable bricks after cleaning the nozzles, shortening the backflushing time and avoiding the hazards of prolonged backflushing leading to large temperature drops in the brick core and easy delamination.

3.5 Slag Control

Before adding diverting sand during ladle hot repair, operate the ladle tilting machine to lower the ladle opening to approximately 45° for slag control. This prevents thin slag from flowing back and clogging the permeable bricks after the ladle is upright, causing poor permeability and affecting production.

3.6 Ladle Bottom Construction

First, use a pneumatic hammer to remove loose bottom bricks. If there are steel sandwiched between different layers of the bottom bricks or if the bottom bricks are cracked, the refractory material must be removed until there are no hidden dangers. Secondly, if the permanent layer around the base bricks has fallen off due to mechanical vibration or damage during the removal operation, all suspended bottom bricks must be removed until the well-sintered permanent layer is visible. Finally, measure the thickness of the remaining bricks. The remaining thickness of the bottom bricks around the permeable bricks and nozzle base bricks should not be less than 200mm. Bottom bricks less than 200mm thick should be removed entirely with a pneumatic hammer.

3.7 Corundum Material Application

Use a mixer to mix the corundum material with water at a weight ratio of 1:0.05–0.08 (1:0.05–0.07 in winter). Use a special measuring bucket to hold the water and wet mix for 5–10 minutes. Use clean water, not wastewater. After mixing, the water and material should not separate and should be fluid. Pour the mixed corundum self-flowing material into the gap between the bottom permeable base brick and the bottom brick. Use a vibrator to vibrate around the permeable base brick twice for 1.5–2 minutes. Through improved quality of the permeable bricks and further standardization of on-site operations, the erosion rate of the permeable bricks significantly decreased, and their lifespan and remaining brick length both improved. See Table 1 for details.

ProjectAverage lifespan/furnace Residual brick length/mm Erosion per furnace/mm
Before Improvement19.819512.3
After Improvement22.121310.4

04 Conclusion

Through the implementation of various measures, the air permeability of the ladle was increased to 99.9%, ensuring the quality of the molten steel and the stability of production. At the same time, the core length of the residual bricks reached 196mm, laying the foundation for further improving the lifespan of the permeable bricks and extending the ladle’s service life.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information