Ladle turnover process: tapping from converter/electric furnace – secondary refining – continuous casting – ladle preparation – waiting for tapping. The normal turnover time is 100~140min depending on the type of steel and continuous casting machine. The tapping temperature of the ladle is 1680-1700℃, the steel storage time is 100~120min, and the typical ladle slag composition (%) for full continuous casting and steel pouring is: Al2O317%~26%, SiO28%~10%, CaO42%~47%, MgO5%~11%, FeO18%~22%. If the process of smelting ultra-low carbon steel such as silicon steel, bridge steel, and automobile plate steel must undergo vacuum treatment, and at the same time, use argon blowing to stir the bottom of the ladle and arc heating in the LF furnace, reducing atmosphere in the furnace, white slag refining, gas stirring and other means to strengthen the comprehensive refining effects such as thermodynamic and kinetic conditions, desulfurization, alloying, and heating. Therefore, the slag basicity range is large, the temperature of the molten steel and slag is higher, the residence time of the molten steel in the ladle is prolonged, the thermal shock resistance is strong, the stirring force is large, and the damage to the lining of the ladle is aggravated.
Causes of damage to ladle refractory materials
1. Ladles are used to transport high-temperature molten steel. During transportation, high-temperature molten steel and slag at around 1680℃ scour and erode them, especially at the slag line, where scouring and erosion are more serious, which is an important factor in determining the service life of a tank.
2. LF and other off-furnace refining treatments seriously damage unfired bricks.
3. When the converter taps steel and molten steel flows out, the lining is subjected to drastic temperature changes, which causes cracks and peeling of the lining material.
4.When the ladle is loaded with molten steel during the converter tapping, the high-temperature molten steel has a strong mechanical scouring on its bottom, causing the lining material in this area to be easily damaged by thermal shock

Damage mechanism of ladle refractory
The damage mechanism of ladle refractory is mainly caused by high-temperature slag erosion and penetration. The slag line of the ladle is mainly melted, and the side wall is cracked and thermally peeled due to the penetration of slag. The melting rate is related to the slag temperature, viscosity and reaction rate of the material. The high temperature of molten steel, the long retention time in the ladle, the low viscosity of slag, and the pore penetration, liquid phase penetration and diffusion in the solid phase of the matrix material cause qualitative changes in the composition and structure of the material surface, forming a metamorphic layer with a high degree of solubility, which is prone to peeling and accelerates the damage of the lining bricks. steel ladle lining refractory with the same or different chemical compositions of refractory materials have different organizational structures and properties, and the damage rate is also different. The ladle cannot operate continuously, resulting in a decrease in the lining temperature or even a cold ladle, which is also prone to lining structure peeling, reducing the service life of the ladle.
The erosion of slag on refractory materials is not limited to the dissolution of the surface, but the slag can also invade (penetrate) the interior of the refractory materials, expand its reaction area and depth, and undergo qualitative changes in its composition and structure near the surface of the material, forming a highly soluble metamorphic layer, which accelerates damage. The proportion of this invasion is roughly proportional to the porosity. Therefore, even if the chemical composition of the refractory materials is the same, their melting loss rates are significantly different due to their different organizational structures.
The higher the open porosity of the refractory material, the faster the slag invasion rate is, and the invasion ratio is approximately proportional to the porosity. Even if the apparent porosity of the refractory materials is the same, the erosion rate will change if the shape, size and distribution of the pores are different.

Characteristics of steel ladle lining refractory material
Based on the above analysis, steel ladle lining refractory materials should have the following characteristics: dense and uniform structure; micro-expansion at high temperature and good volume stability; high strength, and a small ratio of medium-temperature strength to high-temperature strength.
During the use of refractory materials, slag can easily penetrate from the heating surface to the deep inside, significantly reducing the porosity near the working surface and densifying it, forming a very thick metamorphic layer. When the temperature changes drastically, cracks parallel to the working surface are generated at the junction between the metamorphic layer and the original brick layer, causing the bricks to peel off and be damaged. To reduce the structural peeling of refractory materials, the method is to reduce the depth of slag penetration, which can be started from the following aspects:
(1) Improve the slag permeability resistance of refractory materials;
(2) Reduce the porosity of refractory materials and reduce the erosion channel of slag;
(3) The slag reacts with the refractory materials to form a high-melting-point compound retaining wall to prevent the penetration of slag;
(4) Increase the viscosity of the slag. The higher the viscosity of the slag, the worse the erosion of the refractory materials.