Optimizing the converter high manganese hot metal steelmaking process can effectively control the slag overflow and splashing during the operation of the converter and reduce the consumption of steel materials. Thereby reducing the cost of the converter high manganese hot metal steelmaking process, it can effectively improve the utilization rate of manganese in high manganese hot metal, and has outstanding economic benefits.
1 Principle of converter steelmaking process
Converter steelmaking requires blowing O2 into the molten pig iron, which can oxidize the impurities silicon (Si) and manganese (Mn), and release a lot of heat during oxidation. 1% Si can increase the temperature of pig iron by 200℃. In order to ensure that the temperature in the converter meets the steelmaking requirements, converter steelmaking does not require the use of additional fuel. Its main operations are decarbonization, dephosphorization, desulfurization, and deoxidation, which can remove harmful gases and non-metallic inclusions, ensure the converter temperature, and adjust the converter composition.
During the converter steelmaking operation, the smelting purpose is mainly achieved through oxygen supply, slag making, heating, adding deoxidizers, and alloying treatment. The smelting operation can oxidize carbon and other impurities in pig iron to produce steel with better mechanical properties.
2 Analysis of the reaction of Mn in the converter high manganese hot metal steelmaking process
2.1 Reaction of Mn in the converter
In the operation of the converter high manganese hot metal steelmaking process, the reaction process of Mn during the converter blowing is mainly as follows: In the early stage of converter smelting, Mn will be oxidized in large quantities in a short time. Because the binding ability of Mn and O2 is lower than that of Si and O2. Therefore, the oxidation degree of Mn is also lower than that of Si. In the early stage of converter blowing, MnO·SiO2 will be formed, and the CaO content in the furnace will continue to increase, and the following chemical reaction will occur: (MnO·SiO2)+2CaO=(2CaO·SiO2)+(MnO). MnO can be generated after Mn oxidation. MnO can be dissolved in slag, and MnO is in a free state when dissolved in slag. With the converter blowing, the furnace temperature in the middle and late stages continues to rise, and MnO will be reduced. The reaction process at this time is: (MnO) + [C] = [Mn] + {CO} or (MnO) + [Fe] = [Mn] + (FeO).
2.2 Effect of Mn on slag formation in converter–high manganese
During the entire converter steelmaking operation, Mn will have a great impact on the slag deposition process of the converter. The steelmaking reaction itself is an oxidation reaction of elements. When there are differences in the ability of different elements to combine with oxygen, the converter blowing process can be divided according to the order of element oxidation, mainly including early blowing, mid-term blowing and late blowing.
In the early stage of blowing, the oxidation reaction of Si and Mn is relatively intense. During the operation of the converter, the Mn element will react with oxygen to produce MnO. The main function of MnO is to generate low-melting-point compounds with SiO2 and Al2O3 in the slag, including MnO·SiO2, MnO·Al2O3, and 3MnO·Al2O3·3SiO2. After the formation of these substances, the melting point of the slag can be effectively reduced. The specific low-melting-point compounds are shown in Table 1.
| Table 1 MnO low melting point compounds | ||||
| Compound name | MnO ·SiO₂ | 2MnO ·SiO₂ | Mn0 ·Al₂0₃ | 3MnO ·Al₂0₃·3Si0₂ |
| Melting point (℃) | 1291 | 1354 | 1560 | 1195 |
Since the radius of divalent manganese ions and divalent iron ions are similar, both can penetrate the dense layer. MnO has a certain effect on the saturated solubility of CaO. When the content of CaO, FeO and SiO2 in the slag remains at a certain state, the content of MnO will increase. At this time, the saturated solubility of CaO increases, the (C2S+L) two-phase zone shrinks, and the covering layer becomes thinner.
During the operation of the converter, the melting rate of lime will continue to increase. The MnO in the slag will cause the lime to dissolve faster and reduce the degree of return drying. Its slag-reducing effect is more obvious. However, in the actual operation of the converter, if there is no enrichment of FeO and MnO in the slag, there will be obvious excessive slag overflow, and even splashing, which will directly affect the amount of high manganese iron water in the converter and lead to an increase in steelmaking costs.
3 Optimization method of high manganese iron water steelmaking process in converter
In order to reduce the operating cost of the high manganese iron water steelmaking process in the converter, a low-cost and efficient smelting optimization method of high manganese iron water converter was proposed in the research process of the article. In this method, blowing operation, slag management and alloying treatment can be completed. The specific optimization steps are as follows:
3.1 Process parameter requirements–high manganese
In the converter high manganese hot metal steelmaking process, it is necessary to first load hot metal, scrap steel and related auxiliary materials into the converter. The main components of high manganese hot metal and the hot metal temperature are shown in Table 2, and the rest are Fe and unavoidable impurities.
| Table 2 Main components and temperature of high manganese iron water | |||||
| Main ingredients | C | (Si) | (Mn) | (P) | (S) |
| Concentration (wt%) | 4.40~4.63 | 0.35~0.56 | 1~1.35 | 0.091~0.012 | 0.02~0.030 |
| Molten iron temperature (℃) | 1374~1430 | ||||
3.2 Optimization of blowing process
During this operation, a high-pressure, high-speed industrial pure oxygen or air is sprayed on the surface of the molten crude metal using a spray gun, which can oxidize impurities into gases, mainly SO2 and CO. After the gas escapes, the oxides react with the added solvent to form slag, and relatively pure metal can be obtained.
3.2.1 Early stage of blowing
Mainly operated by low gun position and high pressure, the gun position is controlled to 1.2~1.3m, and the oxygen pressure is 0.95~0.92MPa. Low gun position and high oxygen pressure can make the molten pool temperature rise rapidly, shorten the oxidation transition period between Si and C, and reduce the oxidation rate of Mn in the molten iron, so as to reduce the amount and concentration of MnO in the slag. By using direct oxygen blowing operation, the generation rate of FeO can be reduced, the rapid enrichment of FeO in the slag can be avoided, and the fluidity and surface tension of the slag can be effectively controlled to prevent excessive slag overflow and splashing when the carbon-oxygen reaction is more intense.
3.2.2 Mid-stage blowing
Operate using the principle of constant gun and constant pressure. At this time, the free content of MnO in the slag is relatively sufficient, and it has a good slagging effect. In order to increase the replacement speed of MnO, the gun position needs to be controlled at about 1.3~1.4m, and the oxygen pressure is 0.89~0.86MPa. When lifting the gun, it is necessary to pay attention to the appearance of carbon liquid, small pieces of slag flying out of the furnace mouth, and when the concentration of CO is 20%, it is necessary to lift the gun in time. This can make the carbon-oxygen reaction continue, ensure the stability of the heating rate, and increase the replacement speed of MnO. At this time, the slagging situation needs to be controlled in a state of slight anti-drying. In the actual judgment process, the audio curve can run in the lower part of the sickle bend. There are slight slag particles flying out of the nitrogen seal.
3.2.3 Late stage of blowing
That is, 1.5~2min before the end of blowing, slag adjustment operation needs to be carried out according to the actual slagging degree. In the case of a more obvious initial dry state in the later stage, the gun position is 2.0~2.5m, and the oxygen pressure is 0.9~0.92MPa. The holding time of the high gun position and the selection of the gun position are mainly flexibly controlled according to the fire collection situation of the furnace mouth and the concentration curve of CO. It should be noted that during the intervention process, the end point one-pull hit rate should be guaranteed, the reasonable impact depth should be ensured, and the carbon in the molten pool should be prevented from being uneven and high-temperature splashing should be prevented. After the slag adjustment operation is completed, the low gun position is maintained for 10~20s, 1.3~1.5m, which can improve the uniformity of the molten pool, reduce the oxidizability of the slag, delay the slag adjustment time, and increase the holding time of the high gun position and the low gun position during the gun adjustment process, which can ensure the one-pull hit rate of the final slag effect. At the same time, the oxidizability of the slag can be effectively controlled to reduce the secondary oxidation degree of Mn. During the gun pressure operation, the gun position is 0.9m, and the oxygen pressure is controlled at 0.95~0.92MPa. It should be noted that the gun pressure control time is more than 30s.
3.3 Adjustment of slag making system
During the slag making process, the composition and basicity of the slag need to be determined according to the raw material and fuel conditions and the type of iron being smelted. In the slag making management process, it is necessary to strengthen the lime ratio control. Adding lime according to the slag basicity of 2.8 can effectively solve the problem that the slag of high manganese molten iron is highly active, easy to foam, and has low viscosity during the smelting process. This can control the excessive slag overflow and splashing that may occur. Taking advantage of the low temperature and efficient slag formation in the early stage, dephosphorization operation can be carried out through the characteristics of high basicity and high FeO. Because (MnO·SiO2)+2(CaO)=(2CaO·SiO2)+(MnO), the replacement characteristics of the reaction process can be brought into play, the activity and addition ratio of CaO in the slag can be guaranteed, and the MnO in the slag can be kept in a free state, so as to accelerate the replacement of MnO in the medium term and prepare for the formation of slightly anti-dry slag. When controlling the slag formation rate of high manganese molten iron in the early stage, it is necessary to prevent the slag settling rate of high manganese molten iron from being too fast, otherwise the slag and alkalinity may decrease and the temperature may rise too fast. The total amount of lime added to a batch of materials should be maintained at 80%~90%. When the temperature of high manganese molten iron is controlled during the smelting process, the amount of limestone added is also controlled. The cooling efficiency of limestone is 2.0, and the density is relatively light, similar to slag. The characteristics of rapid decomposition of calcium trioxide can be used to remove the gas in the slag layer to achieve the purpose of temperature control, slag control, and increase slag alkalinity. And this method does not use any Fe-containing materials.
3.4 Alloying treatment process
In this operation process, the main purpose is to ensure that the various physical and chemical properties of steel meet the requirements. Alloy additives can be added to the steel to adjust its composition to the specified range. Under certain process conditions, alloying technology can make metals into alloys with certain expected properties. In the actual control of the alloying process, the residual manganese content needs to be controlled. When the proportion of residual manganese content is controlled at 50%, Si and Mn alloys are added according to the principle of low-mix refining and high-filling of slag to prevent the finished product composition from exceeding the standard when the residual manganese content is relatively high. During the smelting operation, if there are obvious slag overflow and splashing problems, the furnace master can notify the alloy worker to retain the alloy or add additives for the second time when tapping the steel to control the performance of the finished steel product and prevent the composition from exceeding the standard.
In the process of this process optimization, when adding the first batch of materials, the total amount of light burning is 80% to 90% lime, and the remaining lime can be added in small batches according to the specific situation of slag reduction. In this way, there is no need to distinguish between different batches of slag materials, and the entire alloying process can also be controlled.
3.5 Optimized process application effect
In the traditional converter high manganese hot metal steelmaking process technology, if the converter smelting method of increasing the residual manganese in the terminal molten steel is simply used for operation, the converter smelting of residual manganese in the molten steel needs to be operated by the low-basicity BaCO3 series slag making process. After adding the BaCO3 series slag making agent, slag making can be carried out. The converter smelting high phosphorus and high manganese hot metal smelting can be operated by the dephosphorization and manganese preservation slag making process. However, the process initially controls the BaO (CaO) -SiO2-FeO slag system, and after blowing for 4.5 minutes, barium carbonate can be produced. However, this method requires the use of Ba series materials, which will lead to an increase in slag making costs. In addition, during the operation of the converter, excessive slag overflow and splashing cannot be effectively controlled.
This process optimization uses conventional slag making agents such as lime and light burning for slag making control. No additional slag making materials are required, and the slag making cost can be effectively controlled. In addition, during the entire process operation, the process operation goals are achieved mainly by relying on the Mn reaction during the converter blowing operation and the influence of Mn on the converter slag forming process. It can reduce MnO in the converter slag, and the power system can propose targeted oxygen supply and slag making optimization systems to improve the overall operation level of the converter.
The excessive slag overflow and splashing problems of high manganese molten iron in the smelting process can be effectively controlled, with a probability of 0%, which can prevent the negative impact of improper smelting operation control on steel consumption. The optimization process controls the residual manganese ratio to 48%~55%, the average content of residual manganese at the end point is increased by more than 0.15%, and the carbon at the end point of the converter is increased by more than 0.015%, breaking through the limitations of the original operation. It can ensure the stability of high manganese molten iron and improve the smelting efficiency. The TFe content in the slag is reduced by at least 1.65%. The process optimization effect is relatively outstanding.
4 Control strategy for steelmaking process of high manganese molten iron in converter
During the process control of high manganese molten iron steelmaking in converter, it is necessary to pay attention to strict control of the entire operation. In particular, before smelting high manganese molten iron, the raw material ratio calculation must be carried out to ensure that the quality and performance of the produced high manganese molten iron meet the requirements of the steelmaking process. After calculating the raw material ratio, put the raw materials into the converter according to the calculated ratio, and heat the high manganese molten iron in the converter to an appropriate temperature.
When controlling the temperature, it is also necessary to adjust it according to different raw materials, usually 1300~1450℃. During the heating operation, it is also necessary to strengthen the control of the amount of O2 input, so as to control the reaction rate in the converter, ensure that the input materials have sufficient time to react completely, and make the quality of the high manganese molten iron reach the expected target.
In the converter smelting production process, it is also necessary to strengthen the titration control, chemical composition detection and temperature control of the high manganese molten iron to further improve the quality of the high manganese molten iron. After the high manganese molten iron reaches the required performance, it is necessary to reduce the temperature in the converter in time, cool the high manganese molten iron, and finally transfer it to the storage container. This is an important control strategy in the operation process of the converter high manganese molten iron steelmaking process.
Strengthening the calculation of raw material ratio, temperature control, titration control, etc. can produce high manganese molten iron that meets the requirements of the steelmaking process. In the subsequent converter smelting operation, it is also necessary to regularly strengthen the physical and chemical properties of raw materials to ensure that high manganese molten iron meets production requirements.
5 Conclusions
In short, the price of high manganese ore is at a low level. Improving the level of high manganese molten iron steelmaking technology can reduce steelmaking costs to a certain extent and ensure the performance of finished steel products. In order to increase the manganese content of molten iron, the residual manganese content at the end of converter blowing can be increased, thereby reducing the production cost of steel enterprises. In the actual operation process, it is necessary to strengthen technical optimization to solve the problems of additional slag making costs for the original Ba-based materials, and slag overflow and splashing in the converter. Through the high manganese molten iron converter low-cost and efficient smelting technology, the residual manganese ratio can be controlled at 48%~55%, the residual manganese content at the end exceeds 0.15%, and the saved Si and Mn gold content is 2.44k/t. The carbon increase at the end of the converter is 0.015%, which can break through the drawbacks of the original operation and ensure low-cost smelting of high manganese molten iron.