Analysis of Damage Causes of 300t Ladle Slide Plate and Technical Improvements to Increase Their Continuous Use Rate

As a functional component for ladle flow control, the slide plate plays a crucial role in the safe operation of the ladle. Abnormal flow control via the slide plate can lead to production interruptions and damage to casting equipment, or even serious safety hazards. In the context of steel plants prioritizing “high efficiency and low cost,” increasing the continuous use rate of ladle slide plates to shorten ladle turnaround time has become an effective cost-reduction measure. Increasing the continuous use rate not only saves on refractory material costs but also reduces labor intensity and tapping temperature. Tan Yongming et al. analyzed the damage mechanism of slide plates, concluding that factors affecting the continuous use of ladle slide plates in multiple heats include slide plate quality, sliding gate mechanism, slide plate installation and operation, and ladle casting operations. Poor control of these factors can all affect the continuous use of slide plates. After implementing measures, the continuous use rate of slide plates increased from 1 set/unit to 1.9 sets/unit. Yu Yanzhong believes that thermal shock, chemical corrosion, and operational factors are the main causes of slide plate damage. He implemented measures regarding slide plate material, mechanical maintenance, installation, and usage, resulting in a reduction of 700 sets of annual consumption while improving the safety of slide plate use. Qiu Wendong analyzed the thermochemical erosion mechanism of aluminum-zirconium-carbon continuous casting slides, concluding that carbon oxidation leads to a porous working layer surface. The reaction of Ca, Mn, and Fe in the molten steel with Al₂O₃ and SiO₂ in the slides generates low-melting-point substances, increasing the pore expansion rate. The decomposition of zirconium mullite further aggravates the chemical reaction by making the slide structure more porous. He also pointed out the development direction of low-silicon, low-carbon, or carbon-free slides. The complex steel grades, long ladle life, and worker operational stability of the No. 3 Steelmaking Plant at Wuhan Iron and Steel Group (WISCO) restrict further improvements in the continuous casting slide utilization rate. This paper discusses related technical issues based on the technical improvement process for increasing the continuous casting slide utilization rate at the No. 3 Steelmaking Plant.

1. Current Status and Damage Causes of Slides

The No. 3 Steelmaking Plant’s continuous casting system is equipped with three 300t combined blowing converters, three 300t refining LF furnaces, two 300± refining RH furnaces, and three “one machine, two strands” slab continuous casting machines. The steel grades cast include pipeline steel, automotive steel, and shipbuilding steel, with a casting temperature of 1530–1580℃ and an average steel volume of 280t. There are 34 ladles, and the integral base bricks, upper sprue, upper slide plate, lower slide plate, and lower sprue together form the steel pouring channel (see Figure 1). The slide plate has an 85mm diameter, and the casting cycle is 37–55 minutes.

Figure 1. Schematic diagram of the ladle channel.

During the use of the ladle slide, phenomena such as steel clamping between slide plates, surface cracks, melting and roughening in the flow interception zone of the lower slide plate occur, limiting the further improvement of the slide plate’s continuous use rate.

Steel clamping sheets with a thickness of approximately 0.3–1.3 mm form around the casting holes of the upper or lower slide plates. The starting point of the clamping sheets is at the position where the slide plate closes tangent to the flow interception zone, mainly present in the flow interception zone of the lower slide plate, as shown in Figure 2(a). The size of the clamping sheets varies depending on the severity of the clamping. Small clamping sheets, approximately 0.3 mm thick, exist within a small area of ​​the flow interception zone of the lower slide plate and are not easily detected; large clamping sheets, approximately 1.3 mm thick, exist throughout the entire slide plate surface, as shown in Figure 2(b). Typically, multiple factors combine to cause steel clamping between slide plates.

Figure 2. Actual image of steel sandwiched between the sliding plates.

The third steelmaking process uses ladle machinery, employing four stacked springs to tightly bond the upper and lower sliding plates together. The surface pressure F = 4KΔx (K: spring force coefficient, Δx: tensile length); the molten steel pressure P = 3.14r²pgh (P: static pressure exerted by the molten steel height on the sliding plates; r: sliding plate radius; p: molten steel density; g: gravitational acceleration; h: height from the molten steel surface to the sliding plates). Calculations show that the spring surface pressure F is significantly greater than the maximum molten steel pressure P. Furthermore, the pressure difference between the four stacked springs is less than 2kN, ensuring uniform surface pressure on both sides of the sliding plates.

During casting, the lower sliding plate’s intercepting area is melted, forming a noticeable obtuse angle. Cracks appear in the lower sliding plate’s travel area; crack propagation leads to melt loss. When the sliding plate closes rapidly, molten steel remaining at the obtuse angle and melted areas of the lower sliding plate is carried into the gap between the sliding plates, forming a sandwiched steel structure.

When the ladle cannot open automatically, oxygen firing is forced. If the slide gate is not fully open, the area around the casting hole on the upper slide gate is easily burned. Repeated and rapid opening and closing of the slide gate during oxygen firing can introduce molten steel into the gap between the slide gates, a phenomenon particularly noticeable with consecutive slide gates. Failure to add priming sand before tapping can prevent the ladle from opening automatically. During oxygen firing, the high-speed oxygen flow swirling in the gap between the upper and lower slide gates can cause the slide gates to burn.

During application, cracks develop on the slide gate surface. Four to five relatively evenly distributed cracks, 0.2 to 1 mm wide, are observed around the casting hole, as shown in Figure 3(a), occurring on both the upper and lower slide gates. Two relatively wider cracks, approximately 0.5 to 1 mm wide and 30 to 50 mm long, are located in the slide gate’s travel direction. These cracks in the lower slide gate’s interception area are easily eroded into grooves after expansion. Two cracks, 0.2 to 0.4 mm wide and extending into the steel strip, are located in the non-travel direction and penetrate the thickness direction. Obvious air intake marks are visible in the non-travel area cracks, as shown in Figure 3(b).

Figure 3. Actual image of a crack on the slide plate surface.

Before use, the slide plate is at a very low temperature. During casting, the slide plate comes into contact with high-temperature molten steel for a short period. The resulting huge temperature gradient causes a strong thermal shock to the slide plate body. Tensile stress is generated outside the casting hole of the slide plate. Once this stress exceeds the strength of the slide plate’s refractory material, radial microcracks will form. These microcracks facilitate the diffusion, accumulation, and penetration of external molten steel, slag, and oxygen, thus inducing accelerated chemical corrosion.

Slide plate melting mainly occurs in the lower slide plate’s intercepting zone. The expansion of the hole in the slide plate’s stroke direction is 90–120 mm. The melted area presents a V-shape, penetrating the thickness direction. However, in some slide plates, the melting does not penetrate the thickness direction, resulting in a fragmented working surface. When the slide plate is pulled apart at the hot repair station, the refractory material in the intercepting zone is easily pulled apart.

Microcracks in the lower slide plate’s intercepting zone propagate into open cracks. During casting, the scouring effect of the flowing steel causes these cracks to propagate further. During the final stages of casting, CaO, MnO, and FeO in the ladle slag react chemically with Al₂O₃ and SiO₂ in the slide gate, producing low-melting-point substances that bind the upper and lower slide gates together. When the slide gates are opened during hot repair, this manifests as slag adhesion, material falling off, or scattering.

Slag adhesion and material falling off the slide gate surface mainly occur in the slide gate’s travel zone, particularly at the lower slide gate’s flow interception area. Observations show that 2-3 mm of the working layer is adhered and removed along its thickness, with the affected area having a diameter of 30-40 mm. This is particularly noticeable in calcium-treated steel and high-manganese steel. During hot repair, this results in difficulty pulling the slide gate, and in some heats, the lower slide gate’s flow interception area is completely dispersed.

Ca and Mn elements in the molten steel react chemically with Al₂O₃ and SiO₂ in the slide gate, generating low-melting-point substances. These substances accelerate the erosion rate of the slide gate. Furthermore, the low-melting-point substances bind the upper and lower slide gates together, making them difficult to pull, leading to roughening and material falling off the slide gate’s working surface.

The erosion of the slide plate is caused by the corrosion of Ca in the molten steel. To improve the castability of the steel, Ca-Al or Ca-Si wires are fed into the molten steel during the refining process, resulting in a horseshoe-shaped slide plate after casting. Ca in the molten steel reacts with Al₂O₃ and SiO₂ in the slide plate to form CaO. CaO further reacts with Al₂O₃ and SiO₂ in the slide plate to form Al-Ca or Al-Si-Ca low-melting-point compounds. The CaO-Al₂O₃-SiO₂ phase diagram shows that 2CaO·Al₂O₃·SiO₂ has a melting point of 1584℃, CaO·Al₂O₃ has a melting point of 1600℃, 3CaO·Al₂O₃ has a melting point of 1539℃, and 12CaO·7Al₂O₃ has a melting point of only 1392℃. These low-melting-point materials form a liquid phase within the casting temperature range. The liquid phase is eroded by the steel flow, leading to pore enlargement. Simultaneously, changes in the calcium content of the slide plate’s working surface affect the refractory material’s microstructure and the slide plate’s service life. Furthermore, when the slide plate opening is low, the high-speed steel flow creates a negative pressure zone between the upper and lower slide plates, as shown in Figure 4. Ca vapor in the molten steel reacts with the absorbed oxygen, and the resulting CaO accumulates on the slide plate surface, exacerbating the slide plate’s chemical corrosion.

3Ca+Al₂O₃ →3CaO+2Al (1)

2Ca+SiO₂ →2CaO+Si (2)

Figure 4. Negative Pressure Zones of the Upper and Lower Slide Plates

The erosion of the slide plate involves Mn corrosion from the molten steel. During casting, the manganese in the molten steel reacts chemically with the refractory material of the slide plate, generating low-melting-point substances. According to the MnO-Al₂O₃-SiO₂ phase diagram, the melting point of MnO·SiO₂ is only 1291℃, while that of MnO·Al₂O₃ is 1720℃. Therefore, reducing the SiO₂ content and increasing the Al₂O₃ content in the slide plate can improve its erosion resistance.

MnO+Al₂O₃→MnO·Al₂O₃(3)

MnO+SiO2→MnO·SiO2(4)

The erosion of the skateboard involves the oxidation of carbon in the slide gate plate. Carbon and graphite in the skateboard begin to oxidize at 450~500℃, and the oxidation intensifies when the temperature exceeds 750℃. The oxidation of carbon or graphite leads to a loose structure of the skateboard. FeO, MnO and other substances in the molten steel or slag diffuse and penetrate into the skateboard through cracks and pores, which accelerates the oxidation of carbon in the slide gate plate. The chemical reactions are as follows:

2C+O₂→2CO(5)

C+O₂→CO₂(6)

FeO+C→Fe+CO(7)

2. Technological improvements to improve the continuous use rate of slide gate plate

One of the important factors affecting the continuous use of slide gate plate is the material and quality of the slide gate plate. Selecting aluminum-carbon zirconium skateboards with good corrosion resistance and thermal shock resistance, and appropriately reducing the SiO₂ content is beneficial to improving the continuous use rate. This type of slide gate plate uses corundum, mullite, and zircon as the main crystalline phases and carbonaceous materials as binders. It has high thermal conductivity, low coefficient of thermal expansion, and fine pores. ZrO₂ can undergo a phase transformation at 1000℃, which is beneficial to improving the thermal shock resistance of the slide gate plate. The optimized physicochemical properties are listed in Table 1.

ProjectBefore OptimizationAfter Optimization
SiO2/%8.15.2
Al2O3/%73.8475
C/%7.17
ZrO2/%5.810
Compressive strength (110℃, 24h) / MPa132.4170
Bulk density (110℃, 24h) / (g·cm⁻³)3.233.25
Apparent porosity (110℃, 24h) / %2.12

Table 1. Physicochemical Properties of Slide Plate Refractory Materials

Selecting a suitable slide plate aperture is crucial. An excessively large aperture will reduce the slide plate opening, and enlarged misaligned holes will result in a larger interception zone. This interception zone is prone to forming dead zones, leading to steel and slag adhesion, thus affecting the safety of the slide plate. According to Bernoulli’s equation, the relationship between the steel throughput, molten steel height, and slide plate aperture is:

In the formula: Q is the steel throughput (t/min); d is the slide gate diameter (m); h is the height of molten steel above the slide gate (m). The steel throughput corresponding to the slide gate diameter is shown in Table 2.

Aperture/mmHeight of slide plate from molten steel surface /m
0.670.700.803.534.07
756.456.587.0314.7715.87
807.347.488.0016.7918.05
827.717.868.4117.6518.97
858.288.459.0318.9720.38
909.299.4710.1321.2622.85

Table 2. Steel Passage (t/min) Corresponding to Slide Plate Orifice Diameter

The permanent layer thickness at the bottom of the ladle in the No. 3 steelmaking process is 180mm, the working layer thickness is 280mm, the distance from the ladle bottom to the slide plate is 673mm, and the residual steel at the bottom of the ladle is calculated as 0.03m. The maximum steel passage of the 85mm orifice slide plate is 8.45t/min, with a total casting time of 33.13min; the maximum steel passage of the 80mm orifice slide plate is 7.48t/min, with a total casting time of 37.43min.

The corresponding slide plate opening for different slide plate orifice diameters is shown in Table 3. Appropriately increasing the slide plate opening and reducing the interception zone area is beneficial to the safe operation of the slide plate. The casting cycle for the No. 3 steelmaking process is 37–55min. Reducing the slide plate orifice diameter from 85mm to 80mm meets the steel casting requirements.

Casting cycle / minSteel throughput / (t·min⁻¹)85 mm aperture80 mm aperture
Slide gate plate interception zone area percentage /%Slide gate plate opening percentage /%Slide gate plate interception zone area percentage /%Slide gate plate opening percentage /%
358.0027501960
407.0030452455
456.2233402850
505.6037353445
555.0942303940

Table 3. Slide Plate Aperture Corresponding to Slide Plate Opening

Based on the Mn and Ca content requirements of steel grades, steel grades are finely classified. Calcium-treated steel can be used consecutively in one heat of ordinary steel; some calcium-treated steels can be used consecutively in one heat of calcium-treated steel; ordinary steel can be used consecutively in two heats of ordinary steel; some steel grades do not allow consecutive use of slide plates.

Other factors affecting the consecutive use of slide plates include the periodic maintenance and upkeep of ladle slide plate machinery, and the regular replacement of ladle machinery with long service lives. During major overhauls, components directly related to surface pressure, such as stacked springs, support rollers, and strip guides, should be given special attention for inspection, maintenance, and replacement.

Strengthen refined operation at hot repair stations, remove residual fire clay from the slide plate chamber, and while pushing and pulling the slide plate throughout the process, observe the slide plate surface for deep scratches, cracks, and abnormal melting phenomena to facilitate slide plate utilization and timely replacement.

To minimize wear, the number of times the slide plate is pulled during steel casting should be reduced. When closing the slide plate, use intermittent operation to avoid rapid opening and closing. Oxygen flow should be standardized; the slide plate must be fully open before oxygen combustion, and the oxygen flow pipe should be vertical. The slide plate should be replaced promptly after the ladle is removed from the production line.

3. Conclusion

(1) Under the background of “high efficiency and low cost” in steelmaking plants, increasing the continuous use rate of the slide plate to shorten ladle turnaround time has become an effective measure. Increasing the continuous use rate of the slide plate can not only save refractory material costs but also reduce labor intensity and tapping temperature.

(2) Steel clamping between slide plates, melting loss in the lower slide plate’s intercepting zone, roughening, slag adhesion, and material falling off affect the safe operation of the slide plate and the improvement of its continuous use rate. Thermal shock, chemical corrosion, and improper operation during ladle opening are the main causes of abnormalities on the slide plate surface.

(3) Thermal shock during ladle pouring causes microcracks around the slide gate opening; Ca and Mn elements in the molten steel or CaO and SiO₂ in the slag react chemically with Al₂O₃ and SiO₂ in the slide gate to generate low-melting-point substances such as MnO·SiO₂ and 12CaO·7Al₂O₃, leading to slag adhesion and material loss on the slide gate; improper flow control can easily cause the slide gate to be burned.

(4) Reducing the slide gate opening diameter from 85mm to 80mm, under the same steel throughput, increases the slide gate opening by 10%, and reduces the lower slide gate interception area by 5% to 7%. The selection of the slide gate opening diameter is very important for the safe operation of the slide gate. Furthermore, through the implementation of measures such as improving the quality of slide gate refractory materials, refining steel grade classification, periodic mechanical maintenance, and refined operation during steel pouring, the continuous utilization rate of the slide gate has increased from 1.67 heats/set to 2.05 heats/set, saving approximately 2500 sets of slide gates annually, resulting in significant economic benefits.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information