Analysis of refractory configuration and refractory erosion mechanism of electric arc furnace lining

The electric arc furnace is an electric furnace that uses the high temperature generated by the electrode arc to melt ores and metals. When the gas discharge forms an arc, the energy is very concentrated, and the temperature of the arc zone is above 3000℃. For smelting metals, the arc furnace has greater process flexibility than other steelmaking furnaces, can effectively remove impurities such as sulfur and phosphorus, the furnace temperature is easy to control, the equipment occupies a small area, and is suitable for the smelting of high-quality alloy steel. The following is the configuration of refractory materials and refractory erosion mechanism of the lining of a 100t ultra-high power electric arc furnace used in a large domestic steel plant.

The 100t ultra-high power arc furnace of a certain steel company is an eccentric furnace bottom steel tapping form. The furnace shell is split, and the upper furnace shell has a water-cooled plate frame structure; the lower furnace shell has a butterfly bottom with a vertical periphery, and the internal masonry refractory forms a molten pool. The furnace shell is used for one standby. After the service life of the furnace expires, the furnace shell is replaced as a whole and rebuilt offline for standby. The refractory materials used in the main parts of the furnace lining are shown in Table 1.

TypeMg0/%Ca0/%SiO₂/%C/%Bulk density/(g.cm³)Compressive strength/MPaFlexural strength/MPa Use location
Magnesia carbon≥76  /  /≥14≥2.9≥35≥8Furnace wall working layer
Brick≥78≥13≤0.6  /≥3.0  /  /Furnace bottom and furnace slope working layer
Ramming≥70≥8≤6  /≥2.0  /  /Repair damaged parts of furnace wall

Analysis of the erosion mechanism of refractory materials for furnace lining

The service life of the furnace lining of a steel electric furnace after its transformation and resumption of production was 300 furnaces, with an output of about 30,000 tons. During the operation, the furnace was protected by wet gunning of the furnace wall and magnesia sand ramming material padding the furnace slope. The consumption of gunning material was 1.7kg/t, the consumption of ramming material was 2.3kg/t, and the cost of refractory materials was 45 yuan/t, which did not reach the ideal service life. The erosion of the refractory materials of the offline furnace lining was dissected and measured, and the erosion of each part is shown in Table 2.

LocationOriginal thickness mmResidual thickness mmErosion thickness mm
Furnace bottom ramming material550350200
Slag line at the electrode hot zone500150350
Slag line in the furnace wall gun area450100350
Other parts of the furnace wall450240210
Furnace slope ramming materialLoss downshift 100 ~ 150mm, sintering layer thickness 200mm

During use, the refractory materials of the furnace lining are subjected to the physical impact of scrap steel charge, the radiation and reflection of the electrode arc, and the chemical erosion of molten steel and slag. Especially at the steel-slag interface, the graphite on the working surface of the magnesia-carbon brick is oxidized by the physical penetration and chemical erosion of the highly oxidizing (FeO content 25% to 30%) slag, forming a loose decarburized structure. After repeated high-temperature oxidation, decarburization, and erosion, it is finally lost in the molten state and flaking state under heat and slag erosion. The lining of the hot zone of the electrode is subjected to high-temperature radiation of the arc, and the lining of the furnace wall cluster oxygen gun area is eroded by the local slag steel circulation, making the lining erosion and damage of these two areas more serious. The furnace bottom and furnace slope are knotted with magnesia sand ramming material. The early furnace masonry knotting is not dense and the furnace sintering is not good. The loose defects of the magnesia sand working layer, under the action of bottom blowing and stirring, the slag infiltrates and reacts with the magnesia sand to form iron-rich magnesia fumite, which reduces the melting point of the magnesia sand and accelerates the dissolution of the magnesia sand. At the same time, when sintering is not sufficient in the early stage of the furnace service, the furnace bottom is affected by collision, vibration and impact of the charge, forming local pits and causing rapid corrosion in some areas.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time