lmm@magnesiacarbonbricklmm.com

Technical support and construction service team

Analysis of the causes of common cracks in ladle slide gate and effective measures to reduce cracks on sliding plates

After use, ladle slide gate will develop cracks in different directions and sizes. The generation of cracks limits the service life of ladle sliding plates and reduces the safety of use. Therefore, refractory and metallurgical researchers hope to reduce the hazards of cracks through various measures. Based on the experience of using ladle sliding plates, the causes of cracks and improvement measures are summarized. In actual use, the crack situation of ladle sliding plates has been significantly improved.

Analysis on the causes of common cracks in ladle slide gate 

Radial cracks

When the slide plate is used, when high-temperature molten steel passes through the cast hole of the slide plate, a huge temperature gradient is formed between the cast hole and the surroundings of the slide plate, causing thermal stress around the cast hole. When the thermal stress exceeds the ultimate strength of the skateboard, radial cracks centered on the casting hole will be formed. This crack is manifested as a “M”-shaped crack formed around the casting hole of the skateboard. This type of crack often occurs and is difficult to control. When such cracks occur, molten steel, slag and oxygen diffuse, gather and penetrate at the cracks, exacerbating chemical erosion. However, since such cracks do not pass through the slideway and other key areas of the skateboard, when the cracks are relatively minor, they will not have much impact on the use of the skateboard. The method of hot embedding steel hoops on the skateboard can control the expansion of cracks and maintain the integrity of the skateboard.

Cracks along the length of the ladle slide gate

The expansion of the crack depends on the shape of the skateboard and the tightening method in the mechanism. The slide gate plate with the two-end tightening method has a certain tensile stress concentration at the outer edges of the two sides of the transverse direction and in the longitudinal sliding direction. This tensile stress that appears in the sliding direction is the main factor that causes longitudinal cracks in the use of the skateboard and promotes the expansion of cracks, which is extremely unfavorable to the life and safety of the slide gate plate. The conical slide gate plate adopts the four-corner diagonal pressure fixing method, which greatly reduces the tensile stress of the slide gate in the longitudinal direction, greatly reduces the possibility of cracks in the slide gate along the sliding direction, and is conducive to improving the safety and service life of the slide gate.

Transverse cracks in the slideway caused by the flatness of the mechanism

Transverse cracks in the slideway are prone to occur in the later stage of the use of the mechanism. When the mechanism is uneven, transverse cracks appear in the slide gate. This type of crack generally occurs in the middle part of the slideway, and most of the cracks appear as obvious cross sections. This type of crack occurs in the core part of the skateboard, that is, the slide area. This type of crack may cause steel to flow between the slide gate surfaces during use. This type of crack is strictly prohibited during the use of the slide gate.

ladle slide gate

Cracks caused by material matching of composite slide plates

There are a large proportion of composite slide plates on the market now. Different composite designs are carried out according to the requirements of different parts of the slide plate during use, which can not only give full play to the advantages of composite materials, but also reduce costs to a certain extent. However, during the use of composite slide plates, if the thermal expansion between the working surface material and the non-working surface material of the slide plate is not well matched, cracks will be generated at the interface due to thermal stress, especially around the casting hole. When this crack is serious, it can cause steel channeling between the ladle slide gate and the nozzle, causing accidents.

Cracks at the board surface and the sub-mouth

After the use of slide plates with sub-mouths, circular cracks are often seen at the edge of the sub-mouth. In production, the contact part between the sub-mouth and the working surface is a weak link. Crack defects are easily formed at this part, and stress concentration will also occur here during use, so cracks are prone to occur. Since this type of crack occurs around the casting hole, it may cause steel seepage accidents along the sub-mouth of the slide plate during use.

Cracks caused by hot repair operation

In the hot repair installation of the drain, the slide crack problem is caused by the drain being installed too tightly. This type of crack mainly manifests as obvious cracks along the joints of the slide gate plate, extending outward to both sides of the slide plate’s width until the slide plate is cross-sectioned. Severe cracks of this type can cause steel to flow between the slide plates.

Effective measures to reduce slide gate plate cracks

In view of the causes of various cracks, measures to limit and reduce cracks are briefly introduced from the aspects of process and operation to achieve the best performance of slide gate plates.

Improve the thermal shock resistance of slide gate plate materials

Practice has proved that by reducing the thermal expansion coefficient and elastic modulus of slide gate plate materials and improving thermal shock resistance, it can effectively alleviate the damage of thermal stress to slide gate plates and reduce the harm of cracks.

Optimize the shape and tightening method of slide gate plates

Optimize the shape and tightening method of slide gate plates, especially the use of finite element method. For example, increase the width of both sides of the casting hole, reduce the width of other parts, and make teardrop-shaped straight line and arc connection, which can make full use of high-quality refractory materials and help reduce thermal stress concentration. For the longitudinal cracks caused by the cooperation of slide gate plates and mechanisms, the fundamental solution is to improve the cooperation between slide gate plates and mechanisms, such as changing from point contact to line contact, from line contact to surface contact, etc., which can greatly reduce the occurrence of such cracks.

Optimize the flatness of the mechanism

When cracks are found due to unevenness of the sliding mechanism, the flatness of the mechanism needs to be tested. If the slide plate and the mechanism are in rigid contact, consider adding a buffer, such as a ceramic pad, to the joint surface to alleviate the problem. During on-site operation, it is necessary to carefully blow the slide plate groove, assembly surface, sliding trolley, frame and mechanism base with compressed air, and press the slide plate lightly with your hand after the slide plate is installed to see if it shakes. Use these methods to determine the fit between the slide plate and the mechanism and confirm whether the fit between the slide plate and the mechanism is flat.

FAQ

Q1: What is the most common cause of cracks in ladle slide gates?

A: The primary cause is thermal shock. When molten steel at temperatures exceeding 1600°C contact the sliding plate, it creates a massive temperature gradient, leading to thermal stress that exceeds the material’s strength, resulting in radial or transverse cracks.

Q2: How can I prevent “Steel Leakage” caused by slide gate cracks?

A: Prevention involves three steps: 1. Ensuring uniform mechanical pressure during installation; 2. Using plates with high thermal shock resistance (like Al-Zr-C); and 3. Implementing proper preheating of the sliding system to reduce the temperature differential during the first opening.

Q3: Does the type of steel being melted affect the sliding plate’s life?

A: Yes, significantly. For example, Calcium-treated steel is highly aggressive toward alumina-based refractories. In such cases, using sliding plates with added zirconia or specialized surface treatments is necessary to resist chemical erosion and subsequent cracking.

Q4: Can the mechanical clamping system cause cracks?

A: Absolutely. If the sliding gate mechanism is distorted or if the clamping pressure is uneven, it creates point loading rather than uniform surface pressure. This mechanical stress often leads to longitudinal cracks even before the steel starts flowing.

Q5: How often should sliding plates be replaced?

A: This depends on the steel grade and plate material. While some high-performance Al-Zr-C plates can last for 3-5 heats, it is critical to inspect for surface roughening and crack width after every heat. If a crack extends to the edge or shows signs of steel penetration, the plate must be replaced immediately.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.