Steel induction furnace is an electric heating device that converts electrical energy into thermal energy by using the principle of electromagnetic induction to induce current inside the metal material in an alternating magnetic field, thereby heating the material until it melts. Induction furnaces are divided into two types according to their structure: coreless induction furnaces and cored induction furnaces. Coreless induction furnaces are widely used because of their fast heating speed, intermittent operation, less element burnout during smelting, and easy use and maintenance. In recent years, high power density, rapid melting, and large-scale development have become the current development trend of coreless induction furnaces.

In the actual production operation process, coreless induction furnace lining will have different types of problems, such as erosion, leakage, slagging, etc. The causes of their formation are as follows:
Erosion
The erosion phenomenon is manifested as thinning of the lining and enlargement of the crucible diameter. The causes of erosion are mechanical erosion and chemical erosion.
1.1 Mechanical erosion
Mechanical erosion is caused by the following reasons:
(1) Collision and friction of the charge.
(2) Electromagnetic stirring. In the area of the Steel induction furnace lining in contact with the molten metal, the molten metal continuously flushes the furnace lining under the action of electromagnetic stirring.
1.2 Chemical erosion
1) Molten metal reaction
The magnesium induction furnace lining has good tolerance to Fe, Mn, and Ni, but weak tolerance to C and Si. At high temperatures, the activity of [C] and [Si] in the molten metal increases, and an interfacial reaction occurs with MgO on the surface of the furnace lining, causing damage to the furnace lining. When using a siliceous furnace lining for melting, SiO2 reacts with [C] in the molten metal as follows: SiO2(s)+2[C]→[Si]+2CO(g). The equilibrium temperature of this reaction for ductile iron smelting is 1467℃, 1540℃ for gray iron, and 1580℃ for malleable cast iron. When the melting temperature exceeds the equilibrium temperature, SiO2 in the furnace lining is reduced by [O], and the furnace lining becomes thinner.
2) Slag erosion
Due to the presence of rust in the charge, unclean return charge, and oxidation of the molten metal at high temperature, a large amount of slag containing FeO is produced. During the smelting process, the viscosity of the molten metal is significantly reduced due to the electromagnetic stirring, and it penetrates into the pores of the lining when it comes into contact with the surface of the lining. At high temperatures, the FeO in the slag reacts with SiO2, Al2O3 or MgO in the lining to produce low-melting-point substances (such as the melting point of FeO·SiO2 is only 1170℃), which are easily melted under the stirring of the high-temperature molten metal and quickly leave the reaction zone and enter the liquid. The greater the difference between the basicity of the lining material and the basicity of the slag, the easier it is for the lining to be corroded.
Leakage
The leakage phenomenon is manifested as metal penetrating into the induction furnace lining. The causes of leakage are:
(1) The furnace density is too low;
(2) The metal has melted before the sintering layer is formed;
(3) Chemical reaction.
Slagging
The slagging phenomenon is manifested as the furnace wall becoming thicker and less smooth. The cause of slagging is the adhesion of metal oxides, return materials containing ions and sand on the furnace wall. The influence of slagging on the furnace lining is manifested as:
① Slagging is the infusible oxides, sulfides or phosphides floating on the molten metal adhering to the parts of the furnace lining where the molten metal flow rate is low and heat loss occurs;
② Reduce the furnace capacity;
③ Reduce the melting efficiency of the furnace;
④ Make the metal hidden in the slag easy to overheat;
⑤ React with the refractory materials of the furnace lining;
⑥ It is easy to cause mechanical damage to the furnace lining during slag cleaning;
⑦ Change the thermodynamic state of the furnace lining in the slag-hanging part.
Quartz sand furnace lining slag, the return material contains more quartz sand (waste sand sticking to the surface of cast iron), these sands will sink to the bottom of the furnace, stick to the furnace wall to make the furnace lining thicker, in serious cases, the furnace bottom will form a V shape, and the furnace volume will become smaller. Quartz sand furnace lining is an acidic furnace lining, and acidic slag will adhere to the acidic furnace lining, especially when the slag line is fixed and the iron tapping temperature is low, the slag line position will be seriously slag, affecting the charging and furnace capacity.
FAQ
In an “all-scrap” electric arc furnace process, how do fluctuations in the composition of the scrap steel accelerate the chemical erosion of the lining?
In-depth analysis: Impurities in the scrap steel (such as low-melting-point metals like zinc, tin, and lead) and surface oxide scale alter the basicity of the slag. If the scrap steel contains a large amount of SiO2 or alumina scale, it will form acidic or modified slag, which reacts chemically with basic refractory materials (such as magnesia or magnesia-alumina) to generate low-melting-point phases. This is precisely the “slagging” process mentioned in the text. Technically, a precise slagging regime (such as controlling the MgO saturation in the slag) is needed to inhibit the dissolution of the brick by the slag.
How does the unique “electromagnetic stirring force” of the induction furnace kinetically exacerbate the erosion process?
In-depth analysis: This stirring force not only accelerates heat conduction but also greatly intensifies mechanical scouring. Kinetically, strong stirring disrupts the saturated diffusion layer on the refractory surface, causing unreacted molten steel to continuously and directly contact the brick surface. Furthermore, the turbulence generated by stirring carries slag deep into the molten metal, increasing the slag/brick contact frequency. Technical countermeasures include optimizing the induction coil frequency or using a refractory matrix with higher densification and stronger high-temperature flexural strength.