Analysis of the Causes of Slag Adhesion in Steel Ladles and Effective Measures to Reduce It

In recent years, severe slag adhesion has been observed on the ladle walls during use, and the slag layer becomes increasingly thicker with the ladle’s age. Slag adhesion reduces the ladle’s volume, lowering the average steel output to 178 tons per heat, and increasing the empty ladle weight from an average of 92 tons to 103 tons. It also hinders the smooth addition of alloy materials and guide sand, negatively impacting production stability. Treating severely slag-adhesive ladles damages the slag line bricks, reducing the ladle’s lifespan, increasing the frequency of minor repairs, and raising refractory material consumption and steel cost per ton. Furthermore, minor repairs often exacerbate slag adhesion, creating a vicious cycle that severely disrupts production. The slag layer is often uneven in thickness and located in different areas, making it difficult to determine the remaining thickness of the ladle lining. Inaccurate thickness assessment can lead to steel leakage accidents. Therefore, reducing or eliminating slag adhesion in the ladle lining is imperative.

01 Analysis of the Causes of Slag Adhesion in Steel Ladles

The working lining of the steel ladle is made of high-alumina bricks containing 88% Al₂O₃. All steel grades are deoxidized using aluminum. The average composition of the top slag of the steel ladle is shown in Table 1.

CaOAl2O3SiO2MgO
37.6738.3413.113.87

As can be seen from the table, the Al₂O₃ content is high and the MgO content is low. Therefore, the phase diagram of the CaO-Al₂O₃-SiO₂ slag system (see Figure 1) with 5% MgO shows that the melting point of the top slag is relatively high. The slag system composition is around 1500-1600°C, indicating a high melting point, while the CaO saturation (CaO/Al₂O₃ = 0.98) is also relatively low. Therefore, during the ladle pouring process, as the molten steel temperature gradually decreases, the top slag solidifies. As pouring continues, the molten steel level drops, and the nearly solidified top slag adheres to the ladle working lining, causing slag adhesion.

Therefore, it can be said that the high content of Al₂O₃, a deoxidation product, in the top slag causes Al₂O₃ to react with the high-alumina brick lining, forming Al₂O₃ deposits. This reduces the ladle volume. Furthermore, with repeated use of the ladle, some slag-adhering material re-enters the ladle, affecting the quality of the molten steel. Simultaneously, the low MgO content in the slag results in a high melting point for the ladle top slag, further exacerbating Al₂O₃ deposition and causing slag adhesion in the ladle. Several secondary factors also contribute to slag adhesion in the ladle, as shown in Table 2.

ProjectReasons for Increased Slag Adhesion:
Converter slag removal* Large slag charge from the converter results in a high content of deoxidation product Al2O3, leading to more severe slag adhesion.
Ladle refining* Low ladle age during LF treatment results in less slag adhesion, while RH and CAS-OB treatments result in more severe slag adhesion.
Steel grades* The large amount of deoxidation products generated during aluminum-killed steel smelting causes more severe slag adhesion.
Ladle turnover* Longer ladle dwell time, i.e., slower ladle turnover, increases the likelihood of slag adhesion.
Ladle cover* Without a ladle cover, the temperature drop of molten steel is large, easily causing slag adhesion.
Insulation layer* Without an insulation layer in the ladle lining, the ladle dissipates heat quickly, easily causing slag adhesion.
Refractory material loss* Damage to the ladle allows slag to enter the damaged area, easily causing slag adhesion.
Ladle minor repair* Poor thermal condition of the ladle after minor repairs easily causes slag adhesion.

02 Measures to Prevent Slag Adhesion in Ladles

Based on the above analysis, to reduce slag adhesion in ladles, the melting point of the top slag must be lowered. From the perspective of increasing MgO, the phase diagram of the CaO-Al₂O₃-SiO₂ slag system with 10% MgO can be studied (see Figure 2). The slag system must be adjusted to fall within the melting point range of 1400-1500°C. While increasing MgO, the saturation of CaO must be maintained; therefore, the CaO/Al₂O₃ ratio must be 1.0, and the MgO content must be between 8-12%.

To adjust the melting point of the top slag, a new type of modifier has been developed. This new modifier uses converter flux quicklime and the undersize of lightly calcined dolomite, mixed in a 2:1 ratio, then briquetteed using a specialized machine. This briquette is added to the ladle during tapping to modify the top slag. The amount of composite briquette added can be dynamically adjusted according to the oxygen content of the tapped steel. The optimal addition method is shown in Table 3.

Oxygen content in steel (ppm)amount of quicklime and lightly calcined dolomite composite balls added (kg)
≤650450-550
650-800550-650
800-1000650-750
>1000700-800

By adding a new type of modifier, the composition of the top slag was stably controlled. The composition of the top slag after adding the new modifier is shown in Table 4. At the same time, the melting point of the top slag was controlled, thus avoiding slag adhesion to the ladle.

CaOAl2O3SiO2MgO
43.3226.389.389.82

The phase diagram of the CaO-Al₂O₃-SiO₂ slag system with 10% MgO content shows that the melting point of the top slag with this composition is between 1400-1500℃. This melting point is relatively low, lower than the temperature of the molten steel in the ladle during casting. Corresponding measures were also taken to address some secondary factors affecting slag adhesion in the ladle, as detailed in Table 5.

CategoriesSpecific measures include:
Steelmaking Process Improving the slag-blocking operation level of the converter tapping process to reduce converter slag entering the ladle;
Controlling the number of ladles in use;
Reducing ladle waiting time;
Strengthening ladle baking;
Ladle InsulationUsing ladle covers;
Using effective ladle insulation agents;
Using heat insulation layers for permanent linings;
Refractory MaterialsImproving masonry quality and controlling brick joint dimensions;
Reducing thermal stress in the lining, improving thermal shock resistance, reducing cracking, and improving the corrosion resistance of RH-impregnated pipe magnesia-chrome bricks, ladle magnesia-carbon bricks, and magnesia-carbon composite materials to reduce melting loss;
Increasing the service life of the ladle bottom and seat bricks, reducing the frequency of minor repairs;
Ladle RepairRepairing obvious melting and spalling areas of the ladle wall promptly to prevent slag and molten steel from seeping in and exacerbating slag adhesion and excessive weight;
Minor Ladle RepairStrengthening baking, and using the ladle for medium and high carbon steel as much as possible after minor repairs.

After implementing the above measures, the slag adhesion in the ladle was significantly improved, the average steel output increased to 186 tons/furnace, and the empty ladle weight decreased to below 93 tons, stabilizing the production rhythm.

03 Conclusion

(1) The main reason for slag adhesion in ladles using high-alumina bricks as working linings is the excessively high content of deoxidation products Al₂O₃, which leads to a high melting point of the ladle top slag. Other factors, such as steelmaking process, steel grade, ladle turnover, ladle insulation, and ladle erosion maintenance, exacerbate slag adhesion.

(2) To reduce ladle slag adhesion, it is necessary to modify the ladle top slag by using composite balls of quicklime and lightly calcined dolomite, adding them to the ladle during tapping. The amount added should be dynamically adjusted according to the oxygen content of the tapped steel, which can significantly reduce the melting point of the top slag. Simultaneously, measures should be taken to reduce converter slag entering the ladle, accelerate ladle turnover, strengthen ladle insulation, and promptly maintain eroded and peeling ladles to alleviate slag adhesion.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information