The phenomenon of steel leakage between the upper nozzle and the upper sliding plate is a common steel leakage failure in the multi-furnace continuous pouring process. It seriously affects the orderly organization of production in this link and even poses a threat to production safety. The following is a guide for the gap between the upper nozzle and the upper sliding plate. An in-depth analysis of the causes of steel leakage and how to effectively improve it.

The upper spout brick squirms toward the inner cavity of the seat brick.
When installing the upper spout brick, apply a layer of fire mud evenly on its outer surface, then squeeze it into the upper spout seat brick, install the upper and lower slide tiles, then lock the sliding frame, and tightly press the upper and lower slide plates, upper sliding plate and the upper spout. Together. If the lining temperature is low, the fire mud cannot harden in a short time. Under the action of the spring pressure, the nozzle brick moves toward the cavity of the seat brick. During the steel pouring process, the fire mud will sinter and shrink, resulting in a reduction in the compression of the spring. , the force between the upper slide gate plate brick and the upper nozzle brick decreases. When the force is reduced to a certain extent, the molten steel will move along the fire mud between the upper nozzle brick and the upper slide gate plate brick under the static pressure of the molten steel. The gap spreads radially to form a ring. When the width and thickness of the ring reach a certain level, steel leakage will occur.
The sealing fire mortar between the upper slide gate plate brick and the upper spout brick is too thick and too thin.
During the steel pouring process, the sintering shrinkage of too thick or too thin fire mud is large, and the porosity of the mud layer after sintering is high, and air easily diffuses into the interior, causing the carbon in the aluminum carbon fire mud to be oxidized, making the fire mud loose. , the strength is reduced and is washed away by the molten steel. Under the action of static pressure, the molten steel passes through the contact surface and causes steel leakage.
The connecting plate is deformed and loose.
During the steel pouring process, the minimum distance between the bottom of the ladle and the liquid level of the tundish is less than 650mm. Affected by the radiation of the high-temperature molten liquid in the tundish, the mounting plate and connecting plate expand, causing the drum to deform and the screw holes in the mounting plate to It is pulled loose under the action of external deformation stress, causing thread slippage. Moreover, during continuous pouring, the friction resistance between the sliding plates is large, and the shear force on the connecting bolts in the horizontal direction increases. During the reciprocating opening and closing movement, the expansion of the bolt hole diameter and slippage are aggravated. When the amount of relative movement between the upper nozzle brick and the upper slide brick reaches a certain level, the fire mud between the contact surfaces will loosen or pulverize, and the molten steel will pass out laterally along the contact surfaces.

(1) Prevent the newly installed water outlet brick from creeping into the seat brick cavity.
After the nozzle bricks are installed, wait for the fire mud to sinter and harden (the waiting time is determined by the temperature of the bottom of the package). If the temperature of the lining is low, bake it to warm it up before installing it.
(2) Prevent the fire mud from being too thick or too thin.
Strictly control the water sensitivity of the fire clay, and when loading the fire clay, it should be exactly level with the bowl mouth of the upper sliding tile and slightly lower than 2~3mm.
(3) Prevent the connecting bolts between the mounting plate and the connecting plate from loosening.
Thicken the thickness of the installation plate from the original 40mm to 55mm (material improvements can also be considered) to increase the resistance to deformation. At the same time, the connecting bolts between the installation plate and the connecting plate are threaded from the bottom of the bag into the bag. The connection method was changed to use counter-channeling countersunk head screws from the inside to the outside of the package, and welding blocks were further added around the connecting plate and the installation plate.