Analysis of the causes of steel leakage in the porous plug brick of the refined steel ladle and the correct solution

The function of the air-permeable porous plug brick is to protect the air-permeable brick core. If the seat brick cracks during use, it will not only fail to effectively protect the brick core and affect its service life, but also cause steel leakage in severe cases. In addition to the quality problems of the seat brick itself, external factors also have a crucial impact on the cracking of the air-permeable seat brick.

The refractory design of the porous plug brick itself is unreasonable

Phenomenon: The seat brick has poor thermal shock resistance, cracks and fractures occur during use, resulting in steel leakage.

Cause: The refractory material design is unreasonable and the thermal shock resistance is poor.

Solutions:

1) Adjust the material ratio of the air-permeable porous plug brick to improve the thermal shock performance;

2) Appropriately increase the amount of steel fiber added, especially for ladles with slow turnover, the improvement effect is obvious.

porous plug brick

External factors cause cracking and steel leakage of the porous plug brick of the air-permeable brick

The opening of the bottom of the installation bag of the overall air-permeable brick is too large

Phenomenon: Due to historical reasons, operating habits, etc., the diameter of the hole at the bottom of the bag is large, reaching 100mm or even larger, which causes the seat brick of the overall air-permeable brick to crack and leak during use.

Reason: The seat brick of the overall air-permeable brick is installed inside the ladle shell, and the tail pipe of the air-permeable brick must extend through the bottom of the ladle shell and connect to the external gas source. There is a mounting hole at the bottom of the ladle, and the diameter of the mounting hole can generally hold the tail pipe 30 to 50mm. During use, the air-permeable brick is in contact with molten steel inside, and the temperature reaches about 1600℃. The bottom is in contact with the outside air and stabilizes at about 150℃. The larger the opening, the faster the bottom of the seat brick cools down, the greater the temperature difference between the top and the bottom, and the seat brick is more likely to produce microcracks under the influence of the temperature gradient. As the number of uses increases, the crack width becomes larger and larger, which may eventually lead to steel leakage accidents. In addition, the depth of the bottom of the air brick core embedded in the base brick is between 0 and 40 mm. When the steel ladle is connected to the steel, the static pressure of the molten steel acts on the brick core and then transmits to the bottom of the base brick. If the base brick is not supported by the steel shell or the support area is small, the 0-40 mm castable is likely to swell and crack under the dual effects of pressure and thermal shock, causing the brick core to move down, which will also cause the air brick to leak steel.

Solution: In this case, the steel plant can be required to plug the hole or open the hole normally as required to ensure the safe use of the air brick.

Uneven bottom of the ladle or deformation of the steel shell

Phenomenon: The uneven bottom of the ladle causes the bottom of the porous plug brick base brick to crack and leak steel. The porous plug brick installed on this severely deformed pad is prone to cracking at the bottom and leaking steel.

Reason: Most steel mills install the porous plug brick directly on the steel shell. Some steel mills lay some leveling materials on the steel shell. Some steel mills used to have too large openings. They used a 10mm thick steel plate to pad the openings and then placed the air bricks. Some steel mills used the steel shells for an extended period of time. The bottom plate or the bottom steel pad has been deformed and uneven due to high temperature, impact of the unpacking machine and other factors. After the air bricks are installed, the bottom of the air bricks and the steel shell at the bottom of the ladle are in point contact, and there is a phenomenon of shaking back and forth. The bottom of the seat brick is uneven, which is equivalent to adding a fulcrum at the bottom of the seat brick. Under the action of thermal shock and static pressure of molten steel, the seat brick is prone to cracks.

Solution: When placing the air brick seat brick, you can use chrome corundum fire clay to level the bottom of the porous plug brick seat brick, and replace the severely deformed pad in time.

Improper replacement method

Phenomenon: There are cracks inside the split porous plug brick, and the brick core falls off and leaks steel during use.

Cause: When some steel mills replace air bricks, they use steel bars from the mouth of the bag to extend to the surface of the brick core and manually pound the brick core down. This operation will inevitably hit the surface of the seat brick during implementation. The strength of the seat brick is very low in the hot state. When it is hit, it may cause damage to the surface seat brick or crack the seat brick. As the cracks expand in the later stage of use, it will cause steel leakage.

Solution: Change the operation method of replacing porous plug brick. It is recommended to use a pulling mechanism to pull out the remaining bricks, which can avoid the occurrence of the above situation and reduce the labor intensity of workers. At present, more and more customers at home and abroad use pulling mechanisms to replace porous plug brick.

The self-flowing material of the expansion joint is not resistant to erosion

Phenomenon: The caulking material filled in the reserved seams around the air brick seat brick erodes too quickly, causing the air brick seat brick to be exposed and cracked.

Reason: In order to facilitate the replacement of the air-permeable brick seat brick, the general design reserves a gap of 40 to 100 mm between the seat brick and the bottom brick, and the castable (or ramming material) is used to seal the seam at this location. If the quality of the material used for filling the seam is poor, it will also affect the use of the air-permeable brick, and in severe cases, it will also cause steel leakage.

Solution: Use high-grade self-flowing material. At present, the main filler used at home and abroad is corundum self-flowing material. Corundum self-flowing material has been adopted by most manufacturers due to its good fluidity, easy construction, and corrosion resistance.

With the rapid development of steel smelting technology today, the refining process outside the furnace has become an important part of the steel smelting process. The correct use of air-permeable bricks can ensure production safety. When using air-permeable bricks, it is necessary to promptly check various hidden dangers, and select reasonable improvement measures for different damage conditions to avoid the occurrence of air-permeable brick steel leakage accidents.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information