In the context of modern steelmaking, out-of-furnace refining technology serves as a vital metallurgical link to improve steel quality by homogenizing molten steel temperature and chemistry and facilitating refining reactions. The implementation of bottom argon blowing in the ladle is a prerequisite for this process. As the key material for gas injection, the porous brick’s performance is of paramount importance for the successful execution of the refining process, quality assurance, and productivity enhancement.
During service, porous plugs are subjected to significant thermal stress caused by large temperature fluctuations and the erosive wear of molten steel, leading to cracking and spalling. In practical applications, transverse cracks frequently appear on the hot face of slit-type corundum-spinel porous plugs in contact with molten steel. This results in detachment at the crack sites, severely shortening the material’s service life. With the trend toward larger ladles, higher smelting temperatures, and extended processing times, the service environment has become increasingly harsh, demanding materials with superior performance and enhanced durability.
Due to their specific location and operating conditions in the ladle, the gas purging success rate and service life of porous plugs have become critical factors limiting overall ladle longevity. Achieving a high purging rate, oxygen-free cleaning, and synchronization with the lifespan of the ladle lining or bottom materials are the common goals of steelmakers, manufacturers, and researchers alike.
By analyzing the wear mechanisms of porous plugs, this paper aims to provide a theoretical basis for researchers to improve the performance of refractories used in these components.

In the steelmaking process, bottom argon blowing through the ladle porous plug is required to facilitate refining and homogenize the temperature and composition of molten steel. Porous plugs for ladles can be classified by their gas channel structure or by their installation method.
There are three main types of porous plugs based on the form of the gas channels: diffused type, straight-hole directional type, and slit directional type.
Porous plugs are divided into two types based on how they are installed: integral type and external-plugging type.
The porous plug is a critical material in the ladle bottom argon blowing process. Its service involves an intermittent cycle: tapping (receiving steel) → gas purging/refining → teeming (casting) → slag dumping → oxygen cleaning. This cycle repeats until the end of the plug’s service life.
Based on its operating environment, the failure of the porous plug is driven by the following factors:
Before use, the ladle is preheated to approximately 1100°C. The tapping temperature from the converter reaches as high as 1640–1700°C, while the temperature drops to about 800°C after teeming. The refractory material on the working face, especially around the gas outlets, is in direct contact with high-temperature molten steel and simultaneously cooled by the continuous gas flow. This creates a massive temperature gradient, subjecting the plug to severe thermal shock, which eventually leads to spalling after multiple cycles.
During argon blowing, the interaction between the high-velocity gas stream and the molten steel creates recirculating flows (eddies). These flows exert impact, scouring, and shear stress on the protruding parts of the porous plug. Additionally, the powerful impact of molten steel on the ladle bottom during tapping accelerates mechanical wear and failure.
Throughout its service, the working face remains in contact with molten steel and slag. Reactions occur between the refractory and the oxides in the steel/slag, forming low-melting-point phases such as FeO·Al2O3,2(MnO)·SiO2·Al2O3,and 12CaO·7Al2O3.These phases are easily washed away by the gas flow, leading to chemical erosion. The penetration and corrosion by molten steel and slag are among the primary causes of damage.
Due to direct contact with high-temperature molten steel, the working face of the porous plug maintains a high temperature, while the non-working face remains relatively cool. During the continuous ladle cycle of receiving steel → refining → casting → hot repairing → receiving steel, the ladle temperature is constantly fluctuating. Consequently, a temperature gradient exists between the working and non-working faces. The existence of this gradient, combined with the different thermal expansion coefficients between the altered layer and the original layer, results in varying levels of volumetric change in each layer. This generates shear stress within the material, inducing transverse cracks that lead to transverse fracturing and the ultimate failure of the porous plug.
Throughout the cycle of receiving steel, refining, casting, slag dumping, and oxygen cleaning, molten steel or slag may penetrate into the slits or cracks caused by thermal stress, leading to slit blockages. Therefore, after the teeming is finished and the slag is dumped, oxygen burning/cleaning must be performed on the porous plug. Because the high-temperature flame directly sprays onto the plug surface, the slag reacts with the refractory material to form low-melting-point phases, causing the plug to melt and form concave depressions (craters). During operation, steel entrapment in the slits and the inability to “blow through” (failed purging) are the primary reasons for frequent replacement of the plugs.
Analysis and Conclusion:
Poor thermal shock resistance is the primary reason for problems such as slit entrapment and spalling in the porous plugs used at Anshan Iron and Steel (Angang). Analysis using ANSYS software demonstrates that the temperature gradient and thermal stress are the root causes of laminar spalling on the working face, which leads to the destruction of the plug.
The thermal shock resistance of the material is a critical factor influencing the erosion and penetration of molten steel and slag. Cracks generated by thermal shock provide channels for the infiltration of steel and slag. Their subsequent reaction with the refractory material leads to structural spalling during periodic use.
Overall, the thermal shock caused by massive temperature differences during the ladle cycle, combined with the erosion and thermal shock destruction from high-velocity gas streams and molten steel during refining, are the primary causes of porous plug failure. As ladles increase in size, smelting temperatures rise, and refining times are extended, the service environment becomes increasingly severe, demanding materials with better performance and longer life. Thermal shock resistance is a decisive factor for service life; thermal cracks allow for the penetration of steel and slag, and the residual steel/slag within these cracks accelerates structural spalling and failure during periodic use. Transverse cracks caused by thermal stress, leading to transverse fractures, are also a major cause of failure. Due to the unique position and service environment of the porous plug in the ladle, its purging success rate and lifespan have become the key factors limiting the improvement of ladle longevity.
Therefore, enhancing the thermal shock resistance of the material will significantly promote the service life of porous plugs, making it a subject highly worthy of in-depth and systematic research.
The primary functions of the ladle bottom argon blowing process are to stir the molten steel, facilitate heating, adjust chemical composition, and remove inclusions to purify the steel. These objectives are achieved through the circulating flow of molten steel driven by continuous argon injection. From the perspective of thermal stress, materials with excellent thermal shock resistance must be selected. Regarding anti-penetration properties, materials that are not easily wetted by molten steel at operating temperatures are preferred. The sequence of wetting angles between oxide refractories and molten steel is ZrO2>Al2O3>MgO.
Corundum-based castables are characterized by high strength and excellent high-temperature performance, making them widely used in ladle linings. However, their high elastic modulus often leads to material spalling. When both corundum and spinel phases coexist in the castable, the thermal shock resistance and high-temperature properties of the specimens are significantly enhanced, thereby improving the overall performance of the castable.
Corundum-spinel refractories consist primarily of corundum and magnesium-aluminate spinel, typically with a high corundum content. Their performance is closely related to the composition, relative content, and particle size of these two phases. Corundum can react with CaO in the slag to form high-melting-point compounds such as CA6 and CA2.This reaction is accompanied by volume expansion, which densifies the material structure. Meanwhile, spinel can absorb FeO and MnO from the slag to form solid solutions, which increases the SiO2content and viscosity of the slag, thereby enhancing the material’s resistance to slag penetration.
The spinel phase in corundum-spinel refractories is generally introduced via two methods:
Ⅰ. Due to the unique position and harsh service environment of porous plugs in the ladle, their purging success rate and service life are the critical factors limiting the improvement of overall ladle longevity.
Ⅱ. The primary causes of porous plug failure are mechanical erosion and thermal shock damage, resulting from high-velocity gas streams and molten steel during operation. Furthermore, steel entrapment in the slits and the inability to “blow through” (purging failure) are the major reasons for frequent plug replacements. Consequently, the performance of materials used for porous plugs requires further optimization and enhancement.
A ladle purging plug is a refractory device installed at the ladle bottom to inject argon gas for stirring and refining molten steel.
Failure is mainly caused by thermal shock, mechanical erosion, chemical corrosion, and clogging from steel and slag penetration.
They offer better thermal shock resistance, slag resistance, and longer service life compared to traditional materials.