In order to improve the life of ladle lining, new materials must be designed in a targeted manner according to the problems existing in the current use process of ladle. The new materials must have excellent thermal shock resistance, and at the same time have certain resistance to desulfurization agent erosion and thermal insulation. In view of the use environment of molten iron, domestic and foreign research and development are mainly based on aluminum carbon. In recent years, aluminum-burned silicon carbide carbon bricks have been widely used in major steel mills due to their excellent thermal shock resistance and erosion resistance. However, because they contain carbon materials such as graphite, the slag line and other parts exposed to the air are easily oxidized, become loose and are the first to be eroded, and the anti-scouring ability drops sharply. At the same time, when containing carbon, the thermal conductivity is high, which easily causes the furnace shell temperature to be high, the heat loss is large, and it is easy to form a lid and bottom, which is very difficult to handle, resulting in passive production. The average temperature drop of the ladle in a steel plant during transportation is about 190℃, which is slightly larger than that of other steel plants. Some steel mills reduce the temperature drop by covering the ladle, but the problem of temperature drop and covering is still prominent in steel plants where the ladle is open and the turnover route is long. According to this situation, clay silicon carbide brick with good matching process for the ladle and excellent related performance have been developed. Its thermal shock resistance and thermal insulation are better than aluminum-chromium silicon carbide brick and aluminum silicon carbide brick.
The main raw materials of clay silicon carbide bricks are coke gemstones, andalusite, Guangxi white mud, silicon carbide, alumina powder, antioxidant is metal silicon, and binder is sulfite pulp waste liquid. The purity of the main raw materials used, coke gemstone, is w(Al2O3)≥43.0%, and the particle size is 3mn~0mm; andalusite w(Al2O3)≥69.0%, and the particle size is 3mm~0mm; Guangxi mud w(Al2O3)≥30.0%, and the particle size is 200 mesh; silicon carbide w(SiC)≥90.0%, and the particle size is 200 mesh; alumina micropowder w(Al2O3)≥99%, and the particle size is 3μm~6μm.
To improve the service life of the ladle lining, the first thing to do is to improve the thermal shock resistance of the working layer bricks. For the thermal stress caused by rapid alternation of hot and cold, a reasonable lining structure should have a better stress buffering and release mechanism to prevent the diffusion of thermal shock microcracks and cause lamellar peeling of the lining. Under thermal shock, for refractory materials containing pores such as aluminum silicon carbide bricks, the generation, expansion and propagation of cracks are related to the fracture surface energy. In order to improve the thermal shock stability of the material, the material should have a high elastic modulus value and a low strength value. The compressive strength of clay silicon carbide bricks is lower than that of aluminum silicon carbide bricks, which is conducive to improving its thermal shock resistance. At the same time, because its apparent porosity is higher than that of aluminum silicon carbide bricks, the evenly distributed pores have a good effect on the buffering and release of thermal stress, greatly reducing the generation of lamellar cracks and lamellar peeling.
Under normal circumstances, since clay silicon carbide bricks have a higher porosity than aluminum silicon carbide bricks, the looser structure will lead to a decrease in its erosion resistance and make it more susceptible to desulfurization agents and slag erosion. However, in actual use, due to its high porosity, the surface is more likely to adhere to the iron slag layer. When the molten iron ladle cools down, the iron slag solidifies in the gap and fills some of the pores. The iron slag layer attached to its surface blocks some of the pores and plays a certain protective and barrier role, ensuring that the clay silicon carbide brick also has good slag resistance. At the same time, the barrier of the iron slag layer avoids the direct impact of high-temperature molten iron on the brick lining and plays a certain buffering role. Reduces the damage to the brick lining caused by thermal shock stress.
The relatively high apparent porosity and low bulk density of clay silicon carbide bricks ensure that it has relatively good thermal insulation performance. The thermal conductivity of gas is the lowest. The evenly distributed pores of clay silicon carbide bricks reduce its thermal conductivity, reduce the temperature drop caused by heat conduction at the bottom and mouth of the molten iron ladle, and help improve the slag and capping phenomenon at the bottom and mouth of the ladle.

Specific applications
When raw aluminum silicon carbide bricks are used in a 150-ton hot metal ladle, the ladle body age is as low as 220 furnaces. During use, the lining was severely peeled off due to thermal shock impact, and the surface was uneven. Densely distributed long and narrow layered cracks were visible in the exposed parts of the brick body. After the clay silicon carbide bricks were put into use, due to their excellent thermal shock resistance, the peeling phenomenon of the brick lining was greatly improved, and the surface of the brick lining was smooth and orderly. At the same time, due to its good thermal insulation, the phenomenon of bottoming and capping of the molten iron ladle is improved, the phenomenon of gun machine packing is reduced, and the mechanical stress damage of the ladle lining is reduced.
Once the clay silicon carbide bricks are put into use in the 150-ton ladle, the average ladle age reaches 350 heats, and the service life is greatly improved. In addition, because the unit price of clay silicon carbide bricks is cheaper than that of aluminum silicon carbide bricks, and because of its low density, light unit weight, low weight per package and long service life, the comprehensive use cost of a 150-ton ladle is significantly higher after it is put into use. reduce. Due to the excellent use effect of clay silicon carbide bricks and significant cost reduction, they have completely replaced aluminum silicon carbide bricks for ladle lining in the 150-ton hot metal ladle system and are still in use today.
Conclusion
Based on the above analysis, the following conclusions are drawn:
(1) Thermal shock is the most important factor leading to damage to the ladle lining. The clay silicon carbide brick developed by the company has excellent thermal shock resistance and can significantly reduce the lamellar cracks and lamellar spalling caused by rapid cooling and heating of a 150-ton iron ladle during transportation and iron receiving.
(2) Clay silicon carbide bricks can ensure relatively good slag resistance after being put into use, and can meet the erosion resistance requirements of the lining to desulfurizers and molten iron slag.
(3) The thermal insulation effect of clay silicon carbide bricks is better than that of aluminum silicon carbide bricks, which improves the phenomenon of 150 tons of molten iron lagging at the bottom and at the mouth.