In recent years, with the development of market economy and social progress, the raw material and labor costs of enterprises remain high, and the development and production and operation of refractory industry are difficult. In addition, refractory resources are becoming increasingly scarce, and people’s concept of saving raw materials and reducing refractory consumption is becoming stronger and stronger. If refractory enterprises want to develop, they must adjust and optimize from many aspects, especially in reducing refractory consumption and reducing costs. However, the refractory industry has many defects in production cost control, mainly manifested as: ① The production and use methods are relatively traditional, relying more on experience to control, and the effect is not ideal. ② Cost control can only analyze the results after the product is used by relying on technical indicators and material consumption statistics, and it is difficult to effectively control in time. Therefore, only by controlling refractory consumption in advance can the competitive advantage of enterprises be enhanced and the enterprises have better development prospects.

Casting technology of ladle working layer
After the ladle lining working layer is used, if all the residual materials of the ladle wall are removed, it will cause waste of refractory materials and increase the cost of the ladle. Therefore, by surface treatment of the residual ladle wall castable, the original material on the ladle wall can be effectively used for the later casting of the new working layer. The amount of original refractory materials retained during removal can save the amount of usage, directly reducing the consumption of ladle refractory materials, and ultimately achieving the purpose of reducing costs.
Casting technology of ladle bottom working layer
Ladle casting has high requirements on the mixing quality of the refractory castables used. During the mixing operation, the mixer is started first and then the materials are placed. The refractory castables are placed strictly according to the rated power of the knotting machine. After placing the materials, dry stir for 1~2 minutes to make the ladle castables evenly mixed, and then add water according to the actual situation of the castables. The amount of water added is determined to be within the range of ±7%. Stir for 2~3 minutes to fully combine the water and the castables to achieve the best quality. The amount of water added affects the performance of the castable. If the amount of water added is too little, the castable’s room temperature pressure resistance is <20MPa; if the amount of water added is too much, the castable will segregate and reduce the castable’s anti-scouring performance. After the castable is stirred evenly according to the dosage, it is evenly fed to the bottom of the ladle, and the vibrating rod is turned on to vibrate while feeding. During the vibration process, two people are required to drag the vibrating rod in the opposite direction at the same time. When there are no bubbles on the surface, the vibration is stopped. This can ensure the bonding strength of the castable. The stirred castable must be poured and vibrated within 30 minutes. The thickness of the knotting of the ladle bottom is determined according to the ladle production process standard. It is generally flush with the air-permeable bricks used. During the knotting process of the ladle bottom, it must be ensured that the bottom of the ladle is flat, the vibration is uniform, there is no honeycomb, and there is no debris on the top. It is static for 30 to 40 minutes until the surface is initially solidified. After the initial solidification strength is met, the casting mold is placed.
Casting technology for the working layer of the ladle wall
The working layer mold is hoisted into the ladle and placed flat and straight. Since the ladle and the mold are used as a set, the deviation of the mold placement is controlled within 10mm. After the mold is seated, it is fixed in time with a tightening rod to prevent the mold from shifting during pouring and vibration. When only the ladle wall is used for bricklaying, the gap between the mold and the original ladle wall is sealed with asbestos felt and other items to avoid leakage during vibration. The castable for the ladle wall is required to have good fluidity. After the castable is stirred normally, the mixer is turned on to the location of the ladle, and the material is evenly fed between the remaining material of the ladle and the mold. At the same time, the vibrating rod is turned on to vibrate while feeding. In this way, there will be no voids inside the castable after vibration, ensuring that the castable is fully combined with the original castable. Stop feeding when the ladle wall castable is tied to the specified height. It is required that the castable vibration must not allow voids, honeycombs, or rough surfaces to appear. The surface of the castable must be vibrated flat, and no water accumulation or uneven height should occur.
Effect of casting on the working layer of the ladle wall
After actual operation, the average amount of refractory castables used when the working layers of 10 ladles were tied as a whole and the average amount of refractory castables used when the 10 working layers were casted for the first three times were statistically analyzed. The statistical data is shown in Table 1. From the statistical comparison, it can be seen that after the ladle wall casting process is implemented, the average amount of refractory castables used for each ladle during construction is reduced by 5.5 tons.
| Working layer construction method | Amount of material used for the bottom of the package (tons) | Amount of material used for the wall of the package (tons) |
| Working layer integral pouring | 4.5 | 9.5 |
| 1st pouring working layer | 1.5 | 4.2 |
| 2nd pouring working layer | 2.2 | 5.2 |
| 3rd pouring working layer | 3.2 | 6.2 |
| Average difference between overall and pouring amount | 2.2 | 3.3 |
Analysis and comparison of the use indexes of the sleeve casting and the integral casting of the working layer of the ladle wall
From January to December 2015, 375 ladles were used, and the statistics were made according to the indicators of the integral casting ladle and the sleeve casting ladle of the working layer. The statistical data are shown in Table 2. In the first quarter, the average index difference between the sleeve casting ladle and the integral casting ladle was 0.4 furnaces, in the second quarter, the average index difference between the sleeve casting ladle and the integral casting ladle was 0.64 furnaces, in the third quarter, the average index difference between the sleeve casting ladle and the integral casting ladle was 0.8 furnaces, and in the fourth quarter, the average index difference between the sleeve casting ladle and the integral casting ladle was 1.2 furnaces. The average index difference between all sleeve casting ladles and all integral casting ladles throughout the year was 0.775 furnaces, and the index difference was less than 1 furnace. It can be seen that the sleeve casting of the steel ladle has little effect on the use of the working layer of the steel ladle and can meet the use requirements.
| Working layer construction method in 2015 | First quarter (furnace) | Second quarter (furnace) | Third quarter (furnace) | Fourth quarter (furnace) |
| Working layer integral pouring | 97.5 | 101.1 | 104.9 | 109.6 |
| 1st pouring working layer | 97.2 | 100.8 | 104.5 | 108.8 |
| 2nd pouring working layer | 97 | 100.1 | 104.6 | 108.4 |
| 3rd pouring working layer | 97.1 | 100.5 | 103.2 | 107.9 |
| Average difference between integral and pouring | 0.4 | 0.64 | 0.8 | 1.2 |
Through production practice on the refining ladle, the ladle castable working layer casting technology is adopted to maximize the effective utilization of refractory materials. At the same time, it will not affect the overall technical indicators of the ladle, and can effectively reduce the consumption of refractory materials in the ladle. Under the premise of reducing the labor intensity of employees, the purpose of reducing the consumption of raw materials is achieved, and good economic and social benefits are achieved.