The steel plant currently has two 200-ton vanadium extraction converters and two 200-ton steelmaking converters. All four converters use the same construction method and an integral taphole, with a taphole life ranging from 80 to 120 cycles. Since commissioning, the steelmaking converters have frequently experienced steel penetration (or leakage) accidents at the taphole, occurring 5-7 times per year. After a taphole penetration occurs, the furnace must be immediately shut down, affecting normal production operations.When the taphole brick is partially damaged, molten steel penetrates through it and reaches the furnace shell area, causing the furnace shell steel plate at the flange-to-shell connection to melt and break through, resulting in slag and steel leakage. After a penetration occurs, a large amount of lime is added to the remaining molten steel to adjust the slag, and then the remaining molten steel in the furnace is poured into the ladle from the large furnace opening to prevent large-area burn-out of the furnace shell. Because the large taphole lacks slag-blocking measures, slag and steel are tapped together, resulting in severe phosphorus reversion in the slag, which easily leads to high phosphorus content in the finished product and burnt-out taphole. After steel leakage occurs at the taphole of the converter, inspection of the taphole channel reveals obvious melting damage to the taphole bricks. Partial cracking of the refractory bricks at the taphole allows molten steel to leak through these cracks, causing leakage. The number of taphole leakage incidents ranges from 49 to 105.
01 Analysis of Steel Piercing Causes
1.1 Taphole Angle
The taphole angle of a converter is typically designed between 0° and 15°. Most steel mills in China use a 0° taphole design, while the Xichang 200-ton converter uses a 10° taphole design. The 10° angle design helps shorten the ladle car’s travel distance during tapping, improving efficiency. However, during tapping, the molten steel cannot fall freely vertically; it moves at an angle within the 10° channel, experiencing a force towards the rear of the furnace. This significantly increases friction, leading to increased stress at the taphole. The vortices formed by the rotating steel flow during tapping exacerbate refractory erosion, easily causing pitting in the taphole channel. The taphole angle design is difficult to improve, requiring other measures to compensate for this defect.
1.2 Bedding Brick Damage
The bedding bricks near the furnace interior exhibit a thinner-than-thicker refractory thickness, making the inner part of the converter a weak point. As the number of smelting furnace cycles increases, the refractory material of the converter body is gradually eroded, and the erosion of the large surface area after the converter causes the thickness of the bedding bricks to gradually decrease. In the middle and late stages of the converter’s service life, due to long-term erosion by molten steel, the thinnest part of the refractory material on the large surface area after the converter is only 300-400mm thick. At this time, the thickness of the bedding bricks inside the taphole is only about 100mm. When subjected to the impact of taphole replacement, the bedding bricks are prone to cracking, and their erosion resistance decreases. To achieve a longer furnace life, methods such as slag splashing, slag coating, and spraying are used to increase the thickness of the taphole and the large surface area back to 700-800mm. At this time, the bedding bricks at the converter taphole are a bonded slag splash layer and a repair material filling layer, and their erosion resistance is significantly lower than that of the bedding bricks. Damage to the bedding bricks is the root cause of steel penetration at the taphole. Damaged taphole bedding bricks are incomplete in shape and have internal cracks, posing a high risk of damage. When maintenance is inadequate, high-temperature molten steel seeps outward from the gaps in the refractory bricks. When this seeps into the molten steel and reacts with the magnesia-carbon bricks in the gaps, the erosion rate accelerates, causing the refractory bricks to become loose, perforated, and damaged.
1.3 Void Water Hammer Effect
During tapping, air bubbles adsorbed on the rough refractory surface rise to the surface. This causes molten steel to fill the areas opposite to where the bubbles have risen, creating an impact that erodes the refractory material. This phenomenon is called void water hammer. The water hammer effect of molten steel has a significant impact on steel penetration at the tapping spout. Once steel penetration occurs at the tapping spout, the refractory bricks are essentially damaged, and the risk of further penetration increases significantly.
From the dissection of the tapping spout area after furnace dismantling, a void penetration channel has formed between the flange connection to the furnace shell and the tapping channel. After the steel is inserted, the hole is re-bored and filled with binding material, then compacted with sprayed refractory material, and finally moistened with sprayed slurry to form a dense binding layer in the previously leaked tapping channel. However, this binding layer is not as dense as that of magnesia-carbon bricks; the base bricks are still essentially riddled with holes. When the furnace lining bricks inside the tapping port are not properly maintained, or when gaps appear between the tapping port and the base bricks, water hammer effects are significant in these gaps, making it very easy for steel leaks to occur again.
1.4 Spraying Process and Repair Material Quality
After the tapping port is replaced, the gaps between the furnace lining bricks, the tapping port base bricks, and the tapping port casing bricks need to be filled with repair material. Refractory material and water are mixed and sprayed through a spray gun to fill the gaps. The spraying process, such as the consistency and spray angle, has a significant impact on the density of the gap filling, thus significantly affecting the number of times the tapping port can be used.The repair material used for filling gaps undergoes boiling and evaporation of water in the residual temperature of the steelmaking converter (around 1000℃), followed by sintering over a period of time to form a dense sintered layer that meets the needs of steel smelting and scouring. The MgO content in the refractory material and the scouring resistance of the sintered material, among other quality indicators, significantly affect the number of times the taphole can be used.
02 Improvement Measures
2.1 Improvement of Post-Converter Liner Maintenance Process
Erosion of the post-converter lining can damage the lining bricks, weakening the refractory’s resistance to erosion. After the post-converter lining is thinned, the refractory material thickened by slag splashing, slag hanging, and spraying has weak erosion resistance. Encountering high-temperature oxidation furnace cycles will exacerbate damage and lead to steel leakage. Therefore, to prevent lining brick damage, the thickness of the post-converter lining should be strictly controlled. To control the degree of erosion, the converter charging amount is controlled within the range of 215±5t, and the scrap steel amount is controlled at 35kg/t. Infrared slag detection is used to prevent slag splashing when steel is not fully tapped, which would cause molten steel to erode the furnace lining.
2.2 Improvement of Liner Brick Quality
The quality of the taphole lining bricks directly affects the use of the converter taphole. Taphole lining bricks made of 98% magnesia were selected, and in actual use, it was found that their erosion resistance was enhanced.
2.3 Improvement of Tunnel Quality
A modular, assembled tunnel casing is selected. During manufacturing, the modular tunnel casing undergoes mechanical compaction, resulting in a higher refractory density compared to integral tunnel casings. Cracked tunnel casings should not be used, as this increases the likelihood of steel leakage. The number of times the tunnel is used should be controlled (≤120 times). When the tunnel is nearing the end of its service life, it should be replaced promptly to prevent localized thinning that could lead to steel penetration.
2.4 Improvement of Spray Irrigation Process
Each boring operation causes the boring head to vibrate and impact the tunnel casing, further damaging the already compromised tunnel. If the grout used for filling after boring is too thick, it will be difficult for the grout to flow back into the damaged casing and gaps, causing steel to become trapped in the tunnel. Therefore, after boring, a thinner slurry should be sprayed to fully fill the voids, ensuring a sintering time of more than 15 minutes. This allows the refractory material to fully solidify and dry, forming a dense, bonded refractory layer.
Daily inspection and maintenance of the taphole are crucial for preventing steel penetration. After tapping, observe the furnace interior of the taphole. Ideally, the distance between the top of the refractory material and the slag splash layer should be 30-50 mm. It should not exceed the slag splash layer. If the furnace interior portion of the taphole is exposed, it must be repaired.
2.5 Improvement of Refractory Material Quality
Improving the quality of the refractory material used for taphole repair is also an important measure to reduce steel leakage at the converter taphole. Currently, a repair material with 80% MgO content is used. To reduce steel penetration, a taphole repair material with 90% MgO content is used, and phosphate is used instead of water glass as the binder. In comparison, the repair material with 90% MgO content showed significantly better erosion resistance than the currently used repair material (80% MgO content). After its implementation, the number of maintenance heats at the converter taphole was reduced from three per shift to one per shift.Furthermore, it is crucial to control the temperature and oxidizing properties of the molten steel. Over-oxidation of the molten steel and high temperatures should be avoided to prevent severe corrosion of the refractory materials. Xichang Steel & Vanadium Plant, through optimizing the converter reblowing process, dynamic heat balance control, and optimizing ladle baking, reduced the tapping temperature from an average of 1678℃ in 2013 to 1654℃ in 2017. Under the same carbon content level, the oxygen content at tapping decreased by 100ppm, which also played a positive role in improving the corrosion resistance of the refractory materials.
03 Results Achieved
By improving the post-boring process of the converter, the converter’s taphole was changed from an integral type to a segmented combination type. Simultaneously, a series of measures were implemented, including increasing the taphole seat bricks, increasing the percentage of MgO in the repair material, and strengthening daily inspection and maintenance. These measures, combined with reducing the oxygen activity of the molten steel at the converter’s endpoint, lowered the converter’s tapping temperature. The rear surface of the converter was stably controlled between 900 and 1000 mm. The number of times steel leaked through the taphole of the steelmaking converter decreased from 5-7 times/year to 0-1 times/year, and the lifespan of the taphole stabilized at around 118 cycles, greatly improving the converter’s smelting efficiency.
04 Conclusion
(1) The design of the converter’s taphole angle, damage to the seat bricks caused by erosion of the rear surface, and unreasonable post-boring process are the main reasons for steel penetration at the converter taphole.
(2) By strengthening the maintenance of the large surface after the converter, standardizing the spraying process after boring, and improving the refractoriness of the seat bricks and repair materials, the corrosion resistance of the refractory materials can be effectively improved, and the number of times the steel is passed through the tap hole can be effectively controlled.