lmm@magnesiacarbonbricklmm.com

What Is Blow Loss in BOF Steelmaking?

During the Basic Oxygen Furnace (BOF) steelmaking process, the steel output is always slightly lower than the total charge of hot metal and scrap. The metal lost during blowing is called blow loss.

Basic Oxygen Furnace

Blow loss mainly consists of the following parts:

Chemical Loss

When hot metal and scrap are refined into molten steel, carbon, phosphorus, and sulfur must be removed. At the same time, silicon and manganese are oxidized, resulting in unavoidable chemical loss.

Dust Loss

In the oxygen jet core area during blowing, iron is oxidized and forms reddish-brown dust particles that are carried away with furnace gas.
Dust loss typically accounts for 0.8%–1.3% of the charged metal.

Iron Oxide Loss in Slag

The slag contains iron oxide (FeO). When slag is removed from the furnace, part of the iron is lost along with it.

Metallic Droplet Loss in Slag

Some molten metal droplets become suspended in the slag, forming iron beads. When slag is poured off, these droplets are also lost.

Slopping Loss

If the BOF operation is not properly controlled, slopping may occur. Molten metal and slag can be ejected out of the converter, causing metal loss.

Slopping loss generally accounts for 0.5%–2.5% of the total charge, depending on raw material conditions and operational control.

Among all types of blow loss:

  • Chemical loss is the largest and unavoidable 
  • Slag iron loss and slopping loss can be minimized through proper operation 

For example, a 50-ton BOF with combined top-bottom blowing producing Q195 steel reported the following blow loss data:

Loss Type Percentage
Chemical loss 4.38%
Iron loss in slag 1.38%
Dust loss 0.71%
Slopping loss 0.96%
Total 7.43%

Why Is Slopping Prevention Important in BOF Operation?

Slopping is a common phenomenon in top-blown converter steelmaking.

Three main types exist:

  • Explosive slopping 
  • Foamy slopping 
  • Metal slopping 

Studies show:

  • Large slopping events can cause 3.6% metal loss 
  • Small slopping events still cause about 1.2% loss 
  • Some research estimates overall losses of 0.5%–5% 

Preventing slopping therefore directly increases steel yield.

In addition, slopping may cause:

  • Severe erosion of converter refractory lining 
  • Steel adhesion on the oxygen lance 
  • Reduced dephosphorization and desulfurization efficiency 
  • Heat loss 
  • Reduced process stability 
  • Limitations on increasing oxygen blowing intensity

For these reasons, slopping control is critical in BOF steelmaking operations.

Root Cause of Explosive Slopping

The fundamental cause of explosive slopping is:

An imbalance in the carbon–oxygen reaction within the molten bath, generating a sudden large volume of CO gas.

During BOF decarburization:

  • The reaction rate is very fast
  • A large amount of CO gas forms instantly
  • Gas expansion violently agitates molten steel and slag

When the decarburization rate reaches 0.4%–0.6%, the CO gas released per second can reach 3–4.5 times the molten steel volume, and its stirring energy is 7–9 times that of the oxygen jet.

Such powerful gas release can eject molten steel and slag out of the furnace mouth, causing explosive slopping.

Another typical scenario occurs when:

  1. The molten bath suddenly cools 
  2. The carbon–oxygen reaction slows
  3. FeO accumulates in the slag 
  4. When temperature rises again (>1470°C) and TFe exceeds 20% 
  5. The carbon reaction restarts violently

This leads to massive CO gas generation and severe slopping.

Principles and Measures to Prevent Explosive Slopping

Prevention Principles

Ⅰ. Control molten bath temperature

  • Avoid excessively low temperature in the early stage
  • Avoid excessively high temperature in the later stage
  • Maintain gradual heating

Ⅱ. Control TFe content in slag

  • Prevent excessive FeO accumulation
  • Avoid over-oxidized slag

Operational Measures

1. Avoid excessive lance height in the early stage

Too high a lance position slows temperature rise and causes excessive TFe accumulation, leading to large slopping when decarburization intensifies.

2. Use small-batch slag additions

Adding slag materials in small, multiple batches helps avoid sudden bath cooling caused by large additions.

3. Avoid excessive fluorite additions

Overuse of fluorite when correcting dry slag may cause early slag formation and FeO accumulation.

4. Control lance lowering timing near endpoint

If the lance is lowered too early while carbon content is still high, rapid decarburization may trigger explosive slopping.

5. Adjust operation in early furnace campaigns

Early campaign furnaces have smaller volumes and lower temperatures, requiring careful control of TFe levels.

6. Pay attention after furnace repair

After refractory repair, the lining temperature is lower, increasing slag oxidation potential.

7. Control residual slag practice

If residual slag contains high TFe and is not properly cooled before hot metal charging, explosive slopping may occur.

Summary rule:

  • Early-stage slopping → low temperature 
  • Mid-stage slopping → high temperature 

How to Adjust the Oxygen Lance When Slopping Occurs

When slopping occurs:

Do not immediately lower the lance.

Lowering the lance increases the decarburization rate and may worsen the slopping.

Recommended actions include:

  • Raise the lance slightly 
  • Reduce carbon oxidation rate
  • Promote gas release from the bath

If the furnace temperature is very high:

  • Add lime to cool the bath
  • Increase slag viscosity to suppress slopping

Other methods include:

  • Adding anti-slopping materials (e.g., insulation board fragments or small wood pieces)
  • Reducing slag TFe content
  • Slightly reducing oxygen flow rate 

Causes and Prevention of Foamy Slopping

Causes

Foamy slopping occurs when:

  • Hot metal contains high Si and P 
  • Slag contains high SiO₂ and P₂O₅ 
  • Slag volume is large
  • TFe content in slag is high

These conditions reduce slag surface tension and create excessive foam, which blocks CO gas escape.

As a result:

  • Slag thickness increases
  • Foamy slag may reach the furnace mouth
  • Slag is pushed out of the converter

Large slag volumes make slopping more likely.

Converters with larger furnace volume ratios generally experience less severe slopping due to better gas escape.

Prevention Measures

Control hot metal composition

  • Reduce Si and P content
  • Use hot metal pretreatment for desiliconization, dephosphorization, and desulfurization.

Adopt secondary slagging

  • Remove early acidic slag during blowing to reduce foaming.

Control TFe in slag

  • Prevent FeO accumulation to avoid excessive slag foaming.

Causes and Prevention of Metal Slopping

Causes

Metal slopping occurs when:

  • Slag TFe content is too low
  • Slag fluidity becomes poor
  • Oxygen jet directly impacts the molten metal surface

CO gas generated during decarburization ejects metal droplets from the bath.

These droplets can adhere to the oxygen lance nozzle, severely affecting cooling and potentially damaging the nozzle.

Metal slopping is also called “dry slag slopping.”

Typical causes include:

  • Prolonged low lance position 
  • Premature second material addition
  • Lowering the lance before slag formation is complete

Prevention Measures

  • Optimize charging practice to avoid excessive bath depth
  • Prevent overcharging 
  • Remove slag buildup caused by slag splashing furnace protection
  • Frequently measure bath level

Most importantly:

  • Maintain proper lance height 
  • Ensure good slag formation 
  • Avoid too low TFe content in slag 

These measures effectively reduce metal slopping.

Slopping usually occurs due to rapid carbon–oxygen reactions, excessive slag foaming, improper lance position, or poor control of slag FeO content.

Operators should slightly raise the oxygen lance, adjust oxygen flow, and stabilize slag conditions instead of lowering the lance.

Effective slopping control improves steel yield, operational stability, refractory life, and production efficiency.

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information