Origin of Alkali Return
Refractory castables, broadly speaking, refer to hydraulic refractory materials composed of refractory granular base materials, powders, and other additives of varying properties. After mixing with water, they are amorphous products with a certain hardness and strength. During construction, they require molds and are poured using vibratory casters. They are widely used in high-temperature industries. If the refractory castable is not dried in time after demolding, white mold may appear on the surface during storage, followed by gradual sanding and pulverization. The sand can then be clearly felt by hand. This phenomenon is called efflorescence, and it is more likely to occur in summer. If measures are not taken promptly, it will significantly affect the quality of the constructed structure.
Causes of Alkali Return
There are many causes of efflorescence, but my personal analysis suggests the main reasons are as follows:
1. The Influence of Alkaline Substances in Raw Materials
The raw materials used in refractory castables contain alkali metal oxides such as Na, K, and Fe₂O₃. When these oxides combine with water and are stirred, they solidify and harden, generating free water that floats on the surface. This water contains loose, colloidal white precipitates. This phenomenon occurs because unhydrated cement particles on the surface of the refractory castable form a saturated solution upon contact with water, subsequently precipitating alumina and hydrated calcium aluminate. This efflorescence is caused by the reaction of alkali metal oxides with carbon dioxide and other substances in the air. Examples of alkali metal oxides in refractory castable raw materials include refractory aggregates, refractory powders, calcium aluminate cement (used as a binder), various silica fume and additives, water-reducing agents, accelerators, and anti-explosion agents. These materials often contain small amounts of alkali metal oxides, some of which are soluble in water, especially the alkali in dispersants, which are almost entirely soluble in water. These alkali metals dissolved in water can migrate to the surface of the hardened body through capillaries. Once on the surface, they react with CO2 in the air to form carbonates, causing alkali return, expansion, and the appearance of white mold, white frost, peeling, loosening, and flaking on the surface of the cast body. The main chemical reaction equations are as follows: Diffusion and reaction of Na+ ions within the castable system:
Na₂O + H₂O → 2Na⁺ + 2OH⁻ 2Na⁺ + 2OH⁻ + CO₂ + H₂O → Na₂CO₃·xH₂O
The carbonate continues to react with the hydration products of aluminate cement:
Na₂CO₃ + CaH₁₀ → CaCO₃ + Na₂O·Al₂O₃ + 10H₂O
The sodium chlorate formed in the above reaction will continue to react in humid air, regenerating sodium carbonate:
CO₂ + Na₂O·Al₂O₃ → Na₂CO₃ + Al₂O₃
2. Porosity and Pore Size
Extensive research on castables based on bauxite cement bonding has revealed that the porosity of the castable is one of the main factors affecting alkalization. The relationship between porosity and water-cement ratio has confirmed the importance of the porosity of the bonding phase.
3. Environmental Humidity
The influence of different environmental humidity levels on the pulverization phenomenon of lightweight castables based on bauxite cement bonding. Clearly, the higher the environmental humidity, the more pronounced the alkalization phenomenon.
Solutions to Alkali Return
(1) Timely Drying of Castables
The key to alkali return in castables lies in the presence of free water. To solve this problem, the free water must be drained in a timely manner, forming stable compounds before alkali metals and alkaline earth metals are converted into hydroxides and migrate, thus preventing alkali return. Therefore, the castable should be baked in a timely manner to drain the free water within it. Based on long-term production experience, I believe the following baking curve can achieve a better baking effect without damaging the already constructed castable and causing unnecessary rework.
(2) Apply an anti-permeability organic coating to the surface of the newly constructed lining layer. If the newly constructed castable cannot be dried in time, a plastic film can be placed over the surface, or an anti-permeability organic coating can be applied to the surface of the newly constructed lining layer and then applied again after 24 hours of curing. This prevents moisture carrying alkali from migrating to the surface. If an anti-permeability organic coating is used, the coating should be colored to distinguish between the coated and uncoated areas. This type of coating generally has an ignition point of around 150℃ and can be completely burned off during equipment operation.
(3) The problem can be solved from the refractory castable itself. The method is to select refractory raw materials with low alkali content, increase the viscosity and speed up hardening of the refractory castable, which can reduce the migration rate of sodium salts. Strengthen quality management, strictly control the amount of water added, and prevent excessive water addition.
Conclusion
The above describes the origin of the alkalization phenomenon of refractory castable and related countermeasures. However, please note that alkali degradation is a natural phenomenon, and it is impossible to completely avoid it using any method. When alkaline degradation has already occurred, the loose portion in the refractory layer is usually less than 10 mm. In this case, the loose material should be brushed off as soon as possible and an anti-permeability coating should be applied.