Factors of Steel Breakout Accidents Between Ladle Slide
1) When pouring calcium-treated molten steel, the calcium and calcium oxide in the molten steel react with the aluminum oxide and silicon dioxide (SiO2) in the aluminum-carbon or aluminum-zirconium-carbon slide bricks, forming low-melting-point products such as 12CaO·7SiO2 and 2CaO·SiO2·Al2O3. These low-melting products are washed away by the molten steel, rapidly reducing the Al2O3 and SiO2 content on the slide brick surface. This leads to excessive wear on the slide brick working surface, resulting in steel inclusions or steel breakouts between the slide bricks.
2) When the oxygen content in the molten steel is high, the carbon and graphite in the slide bricks oxidize, forming a decarburized layer. This increases the porosity and reduces the strength of the slide brick working surface, exacerbating mechanical erosion and chemical attack by the molten steel. The formation of a decarburized layer: Carbon on the surface of the slide plate oxidizes at the pouring temperature (1550-1600°C), forming a decarburized layer. This increases the porosity of the slide plate’s working surface and reduces its strength. When it comes into contact with molten steel, FeO, MnO, and [Ca] in the molten steel diffuse and penetrate into the slide plate through the pores.
3) The molten steel temperature in the ladle after tapping is too high, exceeding 1660°C in some heats. Without external refining to regulate the temperature, this exacerbates thermomechanical and thermochemical corrosion of the sliding nozzle refractory, leading to cracking, steel infiltration, and corrosion-induced steel leakage.
The specific causes may include the following:
1. Sliding gate mechanism
1) The sliding gate mechanism may be significantly deformed due to prolonged use at high temperatures or accidental collisions during operation. This can lead to uneven force distribution between the slide plates, resulting in small gaps in areas with less force distribution, potentially causing steel seepage between the slide plates.
2) The sliding trolley that mounts the lower slide plate may gradually develop misalignment with the upper slide plate mechanism due to prolonged loading and unloading, resulting in a small gap between the upper and lower slide plates.
3) The springs used in the mechanism may deform and fail due to prolonged use in high-temperature environments, even before reaching their service life. Under the static pressure of molten steel, gaps may form between the slide plates, potentially causing steel seepage between the plates. In severe cases, this can lead to steel wear throughout the mechanism.
4) The drain nozzle clamping sleeve may be deformed, causing the drain nozzle to be installed incorrectly. Alternatively, the snap fasteners on the drain nozzle clamping sleeve trolley may wear out due to prolonged use, preventing proper tightening between the drain nozzle and the lower slide plate, resulting in steel seepage. 2. Causes of Slide Plate Problems
1) The surface flatness of the slide plate does not meet requirements; low flatness results in micro-wave gaps between the slide plates.
2) Problems with the slide plate quality. During casting, especially on the secondary slide plate during continuous casting, severe surface scratches or horseshoe-shaped melt damage at the slide plate openings can occur. Molten steel can penetrate into the deeper scratches, where the temperature is relatively low, causing condensation and steel jams. Continued operation of the slide plate, especially during long reciprocating strokes in continuous casting, can widen the gaps between the slide plates due to the jamming, leading to steel leaks.
3. Causes of On-site Operations
1) The refractory mortar is not properly prepared; the consistency is not appropriate. If the mortar is too thin during the nozzle installation, it will squeeze out and provide poor support. If it is too thick, it will not spread properly. Furthermore, when using high-pressure compressed air to blow away residual mortar in the nozzle eye, overly thin refractory mortar can create gaps, creating a risk of steel leaking from the nozzle. 2) Dry refractory sludge inside the upper nozzle mechanism has not been cleaned clean, or there is steel slag. A small amount of refractory sludge is present on the slide surface. Due to negligence during use, the sludge is mixed with granular dry refractory sludge slag when applying sludge to the lower nozzle, which poses numerous production risks.
3) Problems with continuous casting machine operation. After the ladle begins pouring, a large, long nozzle is attached to the lower nozzle for protective pouring. Avoid reciprocating the slide with the large nozzle in place. This can loosen the nozzle due to improper operation, potentially leading to steel seepage. Use a jog mode to adjust the flow rate instead.
Preventative Measures
1. Strengthen the acceptance and inspection of the sliding nozzle mechanism.
1) Before use, carefully measure the slide, a key component of the sliding nozzle, to ensure that all parts meet specified dimensional tolerances.
2) Carefully inspect the sliding mechanism during each ladle operation, replace any deformed or cracked parts, and clean any residual steel or slag from the slide box. 2. Select High-Quality Refractory Materials
1) Refractory materials used in the sliding nozzle must have high high-temperature strength, especially the ladle base bricks. They must withstand mechanical damage during nozzle brick replacement and the erosion of molten steel, and must last the entire life of the ladle lining.
2) They must have excellent thermal shock resistance and resist cracking during use.
3) They must have a high load softening point and excellent oxidation resistance, ensuring the aperture remains stable during use and free of dents, pitting, or roughness.
3. Optimize Operations
1) Strengthen process control and carefully inspect refractory materials to ensure both their appearance and internal quality.
2) Clean any residual steel and mud from the inner cavities of the nozzle and base bricks, refill with drainage sand, increase the automatic pouring rate, and avoid oxygen-burning pouring.
3) Close the sliding nozzle promptly after the ladle is completely poured to prevent slag from flowing into the nozzle. 4) Adjust the hardness and amount of refractory clay based on the diameter expansion of the base brick and upper nozzle brick, as well as the depth of the upper nozzle brick recessed into the base base plate.
5) Accelerate the ladle’s turnover to reduce thermal shock damage to the ladle’s refractory materials.
6) Install the slide plate in strict accordance with operating instructions. Clean debris from the mold frame, the working surface, and the back of the slide plate. Keep the slide plate fully open during oxygen firing.
7) Ensure effective smelting process control to ensure the final molten steel temperature and strictly control the oxygen and calcium content at the final stage of the molten steel.