lmm@magnesiacarbonbricklmm.com

Technical support and construction service team

Configuration and Construction Method of Refractory Materials for Tundish in Small Billet Continuous Casting

The refractory materials in the tundish of small billet continuous casting machines suffer from problems such as short tundish lifespan and frequent refractory material accidents, significantly impacting production and quality stability. With accelerated transformation and upgrading, higher demands are placed on billet output and quality improvement, among which the stability of tundish refractory materials plays a crucial role. Therefore, optimizing tundish refractory materials, improving their stability and service life, and ensuring stable and smooth continuous casting production are particularly important.

01 Small Billet Continuous Casting Parameters and Tundish Refractory Material Configuration

The production and use of tundishes require various refractory materials, including castables, coatings, dry refractory materials, nozzles, slag retaining wall series, and the three main components of continuous casting. The refractory materials in the tundish of small billet continuous casting machines are no exception. The main configuration of tundish refractory materials is shown in Table 1, and the main parameters of the continuous casting machine are shown in Table 2.

Table 1 Main Configuration of Tundish Refractory Materials for Billet Continuous Casting

ProjectMaterial
Integral castable liningHigh Alumina
Working layer (slag line area)Magnesium
Impact plateHigh Alumina
Stop rodAluminum-Carbon/Magnesium-Carbon
Slag retaining wallMagnesium Preform
Sprue seat brickHigh Alumina/Aluminum-Carbon
Inlet nozzleInlaid Aluminum-Carbon Zirconia Gate
Large nozzleAluminum-Carbon
CoverHigh Alumina
Integral nozzleHigh Alumina/Aluminum-Carbon/Chromium

Table 2 Main parameters of billet continuous casting machine

Casting machine numberCasting machine flow rate / flowCasting machine basic radius / mTundish capacity / tCasting machine metallurgical length / mMolten steel superheat / ℃Working speed / m·min−1Ladle molten steel weight/ tThroughput / t·min−1
Machine No. 1610323520~351.8~2.21202.16~2.63
Machine No. 2610323520~351.8~2.21202.16~2.63
Machine No. 359303220~352.2~2.61202.19~2.69

02 Tundish Refractory Material Optimization

2.1 Refractory Material Parameter Optimization

2.1.1 Stopper Rod Optimization

The flow control method for small billet casting machines is stopper rod control. The original stopper rods for small billets had a thick, blunt head, resulting in a large contact area with the steel flow and the inlet nozzle during flow control. Under the same steel throughput conditions, the erosion rate was fast, and with increasing ladle age, steel loss due to excessively rapid rod head erosion was prone to occur. Therefore, the stopper rod selection was optimized. The stopper rod head was improved to a thinner, pointed head, and the length was increased by 20mm. The R-value of the stopper rod head was optimized, expanding the effective flow control contact area, improving service life, improving erosion uniformity, and improving flow control accuracy, ensuring good flow control in later stages. The center process hole of the stopper rod was extended to improve the thermal shock stability of the rod tip. The total length of the stopper rod was increased by 100mm, making the stopper rod higher than the tundish cover, preventing the stopper rod core from deforming during baking and the nut from loosening, reducing flow control anomalies. After optimization, the stopper rod head and the inlet nozzle dimensions are better matched, resulting in stable flow control.

2.1.2 Optimization of the Inlet Gate

The original inlet gate for small billets had an inner diameter of approximately 30mm. This resulted in a large steel flow rate per unit time, requiring frequent intervention of the stopper rod for flow control at low casting speeds. This increased the number of times the stopper rod was jammed, which was detrimental to its lifespan and could lead to the stopper rod failing to lock properly when casting was stopped. While reducing the inner diameter of the inlet gate to a certain level (e.g., approximately 23mm) significantly improved flow control, it also caused problems with insufficient steel flow when replacing the submerged entry gate. After numerous experiments, an inlet gate with an inner diameter of approximately 25mm was found to be most beneficial for steel flow control and improving stopper rod lifespan. The experimental tracking and comparison results are shown in Table 3.

Table 3 Results of the nozzle test

Serial Number Package Number Number of FurnacesⅠⅡⅢⅣⅤWater inlet diameter/mmAbnormal Remarks
StrokeMinimum steel flowStrokeMinimum steel flowStrokeMinimum steel flowStrokeMinimum steel flowStrokeMinimum steel flow
172628Stuck26Stuck25Stuck23Stuck26Stuck23None
202625Stuck23Stuck27Stuck24Stuck23Stuck23Steel flow cannot keep up when changing the inlet
332826Stuck25Stuck23Stuck27Stuck24Stuck23None
462722Stuck22Stuck21Stuck25Stuck22Stuck23Steel flow cannot keep up when changing the inlet
592724Stuck23Stuck22Stuck21Stuck23Stuck23None
692728Stuck26Stuck25Stuck23Stuck26Stuck25None
732925Stuck23Stuck27Stuck24Stuck23Stuck25None
872626Stuck25Stuck23Stuck27Stuck24Stuck25None
962722Stuck22Stuck21Stuck25Stuck22Stuck25None
1002824Stuck23Stuck22Stuck21Stuck23Stuck25None

2.1.3 Impact Plate Optimization

Impact plates are used in the tundish steel impact zone to prevent bottom leakage accidents. The original impact plate for billets was 480mm×480mm×60mm (length×width×thickness), which was too small and insufficient in thickness, resulting in inadequate impact resistance. If the long nozzle is not properly aligned or the ladle is tilted, the steel flow can easily impact areas outside the impact plate, affecting the tundish’s service life and, in severe cases, causing bottom leakage accidents. Therefore, the impact plate was redesigned with dimensions of 700mm×550mm×100mm (length×width×thickness). To facilitate placement close to the overflow outlet wall, the corresponding area was designed as a small trapezoid, as shown in Figure 1.

Figure 1 Schematic diagram of the improved impact plate

2.2 Optimization of Refractory Construction Methods

2.2.1 Improvement of Nozzle Seat Brick Construction Method

In tundishes using refractory coating, the area around the nozzle seat brick is filled with refractory material after installation to ensure its stability. Because the refractory material contains a large amount of moisture, the nozzle seat brick absorbs this moisture. Before steel pouring from the tundish, insufficient drying time or inadequate drying temperature often leads to incomplete moisture removal from the nozzle seat brick. This results in cracking or bursting when receiving molten steel from the ladle, causing the nozzle to sink. This leads to the stopper rod losing its flow control function or severe scouring, affecting the number of heats that can be poured consecutively from the tundish, and in severe cases, hindering the smooth progress of continuous casting.

To address these shortcomings, a new nozzle seat brick construction method has been developed. Specifically, the process involves: Before construction, reserving space at the bottom of the tundish for installing the nozzle seat bricks. After the remaining areas at the bottom of the tundish are coated with a mortar, the nozzle seat bricks are installed as required. Then, magnesia-based dry vibratory mortar is used to fill the area around the nozzle seat bricks, and the mortar is compacted using a small hammer. The main components of the dry vibratory mortar include sintered magnesia particles of different sizes, fused magnesia fine powder, phenolic resin powder, and a small amount of additives. The dry vibratory mortar contains no moisture, making the nozzle seat bricks less prone to cracking during steel pouring. The filled dry vibratory mortar does not form a unified structure with the nozzle seat bricks and the permanent layer at the bottom of the tundish during high-temperature sintering, allowing it to automatically separate and detach when the tundish is tilted after pouring. This effectively prevents the tundish nozzle seat bricks from cracking or bursting during steel pouring, facilitating the normal flow control function of the stopper rod and solving the problem of insufficient continuous pouring capacity due to severe stopper rod erosion. Furthermore, the nozzle seat bricks automatically separate and detach when the tundish is tilted after pouring.

2.2.2 Optimization of the Inlet Gate Installation Method

After the tundish working layer coating is applied to the billet, the inlet gate is installed immediately. Because the coating contains a large amount of moisture, the inlet gate will absorb moisture from the coating during subsequent construction and use. This moisture absorption can easily lead to cracking and other problems, affecting steel flow control and even disrupting smooth production. Therefore, the inlet gate installation method has been optimized. It is now required that the working layer coating be left to dry naturally for 3-5 hours before installing the inlet gate.

2.3 Optimization of Refractory Material Use

2.3.1 Optimization of Inlet Gate Baking Process

Traditional billet inlet gate baking devices use a dedicated baking machine. The baking machine flame surrounds the inlet gate, slowly heating it to the required temperature. This method has low baking efficiency and is detrimental to the inlet bowl and tundish shell. Furthermore, during the overall inlet gate baking process, collisions with the baking machine can cause inlet gate breakage. The billet sprue baking process was improved from external baking to internal exhaust baking. The flame is extracted from the bottom of the tundish, and the sprue is baked from the inside out. The baking device is simple, easy to operate, and produces better baking results.

2.3.2 Tundish Baking Process Optimization

The tundish baking time is generally too long (average 5-7 hours), resulting in over-baking of the stopper rod, reducing its lifespan, and repeatedly causing the stopper rod to stick to the sprue due to over-baking. Through a series of optimizations and adjustments, a tundish baking time of 3-5 hours is sufficient to meet the conditions for casting. For tundishes with excessively long baking times, the number of furnaces used must be limited or the tundish scrapped, establishing a fixed standard. The flame requirements for the tundish baking process are as follows: (Small flame time: flame touches the bottom of the tundish; Medium flame time: blue flame overflows the tundish cover by approximately 500mm; Large flame time: blue flame overflows the tundish cover by approximately 300mm; Minimum abnormal time: cancel or reduce medium flame time; Maximum abnormal time: increase small and medium flame time).

2.3.3 Optimization of Casting and Gate Replacement Operations

Before casting, billet operators are accustomed to repeatedly testing and inspecting the stopper rods, which can easily damage the anti-oxidation coating on the stopper rod head. During the casting process, some employees also have a habit of rushing the stopper rod, which can easily lead to cracking of the zirconia cup at the top of the gate, accelerated rod head wear, and increased stopper rod accidents. Therefore, the casting operation mode has been changed, requiring gentle rod handling to avoid jamming, prohibiting rushing the rod, and requiring quick replacement of the submersible gate to prevent the stopper rod from jamming. Furthermore, changing the gate while the steel flow is continuous helps reduce wear between the stopper rod head and the top of the gate bowl.

03. Effects of Refractory Technology Optimization Application

1) The average ladle life of Units 2 and 3 in 2018 was improved compared to 2017, with Unit 3 showing a significant increase of 56.60%, and the highest ladle life increasing from 18 heats to 30 heats.

2) Billet refractory accidents were significantly reduced. The rate of planned shutdowns due to billet refractory issues increased from 85.72% in 2017 to 95.91% in 2018. The number of unplanned shutdowns due to refractory issues decreased from 14 in 2017 to 6 in 2018.

3) Tundish baking time was significantly reduced from 5-7 hours to 3-5 hours.

04. Conclusion

The overall design of billet refractory materials was optimized, and the tundish refractory standards applicable to billet continuous casting were determined and solidified. The construction method for billet refractory materials has been improved, solving a series of problems such as sinking of the sprue seat brick and cracking of the upper sprue. This has improved the stability of the refractory materials used in the tundish and perfected the billet refractory material usage process, thus extending the service life of the refractory materials.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.