1. Selecting an Appropriate Refining Slag System
Generally speaking, refining slag systems are required not only for deoxidation but also for desulfurization, inclusion adsorption, and submerged arc slag formation. To reduce oxygen content, increasing slag basicity can lower the equilibrium oxygen content in steel and increase the sulfur distribution ratio between slag and steel, thus facilitating both deoxidation and desulfurization. High-basicity slag systems are preferred, but the basicity of the refining slag should be kept within a reasonable range. Excessive basicity, for example, exceeding 5.0, increases the melting point of the refining slag, slows slagging, and compromises deoxidation and desulfurization performance. Therefore, high-basicity refining slag is not recommended. Practice has shown that a slag basicity of 2.5-3.0 provides excellent deoxidation and desulfurization capabilities, as well as good inclusion adsorption and submerged arc performance.
2. Control of Argon Blowing in the Ladle
The functions of argon agitation are: first, it removes dissolved oxygen from the steel; second, it flots the deoxidized products, thereby achieving their removal.
1) Dissolved Oxygen Removal by Argon Blowing During the smelting process, argon is continuously blown in through the permeable bricks at the bottom of the ladle. The bubbles act as a small vacuum chamber in the molten steel. As the bubbles rise, they agitate the molten steel, causing the dissolved oxygen in the molten steel to diffuse into the argon bubbles, thereby achieving the desired removal effect.
2) Inclusion Removal by Argon Blowing in the Ladle Under argon blowing conditions, the removal of solid-phase inclusions in steel relies primarily on the flotation of small bubbles. Inclusions collide with small bubbles, adhere to the bubble walls, and then float up with the bubbles for removal. The probability P of an inclusion being captured by a bubble is equal to the product of the probability PC of an inclusion-bubble collision and the probability PA of the inclusion being adsorbed on a bubble after the collision. A foreign study showed that when the contact angle between solid particles and the solution is greater than 90 degrees, nearly all particles reaching the bubble surface adhere to the bubble, regardless of the contact angle. When the contact angle is less than 90 degrees, the adhesion rate decreases sharply as the contact angle decreases. The contact angles of Al2O3 with SiO2 and molten steel are 144 degrees and 115 degrees, respectively, indicating that they are not wetted by the molten steel. Therefore, they easily adhere to bubbles in the steel. Therefore, the efficiency of removing inclusions from steel is primarily determined by the probability of their collision with bubbles, with the probability of large inclusions colliding with bubbles being much greater than that of small inclusions. Furthermore, the probability of inclusions being captured by bubbles is also determined by the number and size of bubbles blown into the molten steel. The greater the number of bubbles blown in and the smaller their size, the greater the number of inclusions removed. The size of the bubbles produced by argon blowing is primarily determined by the argon flow rate or intensity. The greater the argon flow rate, the larger the bubbles will be when they leave the blowing element. Therefore, using low-intensity argon blowing (i.e., soft argon blowing) and appropriately extending the blowing time can facilitate inclusion removal. Alternatively, using multiple blowing elements to simultaneously blow argon can introduce more small bubbles into the molten steel within the limited purge time.
3) Inert Protective Atmosphere During Ladle Argon Blowing: Argon is blown throughout the ladle smelting process. Argon is an inert gas with a greater density than air. After escaping from the molten steel, it coats the steel surface, forming a protective atmosphere that prevents secondary oxidation and thus reduces the oxygen content in the molten steel.
3. The Impact of Refractory Selection on Oxygen Content
Some of the oxygen in steel is absorbed into the molten steel through erosion of the refractory, so refractory materials must possess good resistance to rapid cooling and heating. Ladle refining is generally an intermittent operation with large temperature fluctuations. Argon is also blown throughout the process, which has a strong scouring effect on the furnace lining. Therefore, refractory materials must possess excellent high-temperature strength.
4. Control of AlS Content in Steel
The AlS content in steel has a significant impact on oxygen content. When the AlS content is controlled at 0.015%, the oxygen content in the steel does not decrease significantly with increasing AlS content. However, when the AlS content is controlled at 0.030%, the oxygen content in the steel remains essentially unchanged. Furthermore, when the aluminum content in steel exceeds 0.030%, the aluminum in the steel easily combines with oxygen in the slag, reducing compounds such as SiO2 and MnO in the slag, increasing the amount of Al2O3 accumulated in the molten steel. Too much aluminum will greatly increase the secondary oxidation of the molten steel during pouring, resulting in Al2O3 inclusions remaining in the finished product. Therefore, it is more appropriate to control the residual aluminum content at 0.015% to 0.030%.