5 Effective Measures to Reduce Converter Lining Erosion and Extend Converter Refractory Life

Converter lining erosion is one of the key factors affecting converter campaign life, steelmaking productivity, and refractory consumption costs. During oxygen blowing, the converter lining is continuously exposed to severe thermal shock, molten steel and slag corrosion, mechanical impact, and intense chemical reactions. If local damage develops too quickly, it can threaten furnace safety, increase maintenance frequency, and shorten converter service life.

For modern steel plants, improving converter refractory life and reducing the erosion rate of the converter lining have become important goals for lowering steelmaking costs and stabilizing production. Therefore, steelmakers are increasingly adopting advanced converter lining maintenance technologies, optimized slag splashing techniques, and high-performance magnesia carbon bricks to achieve longer campaign life and better operational efficiency.

To ensure the safety and stability of refractory materials throughout the furnace campaign, rapid damage to localized areas of the lining must be avoided. Strengthening daily monitoring and timely repair of severely eroded areas helps balance the wear degree of each section of the furnace lining and effectively prolongs converter life.

Traditional maintenance methods mainly include brick replacement, gunning repair, slag splashing, material replenishment, and slag retention. However, these methods often require converter shutdowns and sufficient sintering time, which can negatively affect productivity and operating costs. By applying comprehensive converter lining protection technologies, steel plants can significantly reduce erosion rates, improve production efficiency, and lower refractory consumption.

Optimized Molten Pool Structure Design for Converter Lining Protection

During the converter blowing process, extremely complex oxidation and reduction reactions occur simultaneously with high-speed molten bath movement. Throughout furnace operation, different areas of the converter lining experience varying levels of chemical corrosion, thermal stress, and mechanical impact. As a result, erosion rates differ greatly across different furnace sections, leading to uneven converter lining life.

To solve this issue, the original converter design was optimized based on actual erosion conditions in different areas of the furnace lining. A specially designed steelmaking converter lining structure was adopted to improve overall refractory performance and operational stability.

The converter working layer uses multi-layer magnesia carbon bricks with a gradually thickened transition design in the lower molten pool area. The length of the annular MgO-C bricks gradually increases from the upper layer to the lower layer, meaning the thickness of the molten pool refractory gradually increases downward while the converter inner diameter gradually decreases.

Integral structure of refractory brick lining for converter

This special design forms a conical molten pool structure with a wider upper section and narrower lower section.

During converter operation, especially during oxygen blowing, severe erosion commonly occurs in the molten pool and bottom slag line area. These sections often become weak points during the later stages of converter operation and represent major safety risks.

The optimized lining structure effectively addresses rapid erosion in vulnerable areas. By using multi-layer annular magnesia carbon refractory bricks, the converter achieves better wear balance, improved structural stability, and more economical maintenance throughout the entire furnace campaign. This design not only enhances furnace safety but also significantly extends converter refractory service life and improves economic performance.

Innovative Slag Splashing Technology to Extend Converter Campaign Life

Traditional slag splashing protection methods have been further optimized to improve the effectiveness of converter lining maintenance.

In the improved slag splashing process, the oxygen lance no longer continuously blows nitrogen gas. Instead, nitrogen injection is applied intermittently during slag splashing operations. Under the impact of high-pressure nitrogen, liquid slag forms strong waves and splashes repeatedly onto the converter lining surface, where it adheres, solidifies, and forms a protective slag coating.

High-viscosity final slag with strong refractoriness is repeatedly deposited onto the converter lining under high-pressure nitrogen impact. This significantly improves the effectiveness of slag splashing furnace protection and enhances refractory coating stability.

Without adding special equipment, increasing labor intensity, or extending production rhythm, the optimized slag splashing process greatly improves converter protection efficiency. At the same time, it effectively slows the erosion rate in the molten pool area and reduces refractory consumption costs.

Compared with conventional maintenance methods, optimized slag splashing technology offers a more economical and efficient solution for prolonging converter lining life and reducing steelmaking downtime.

Iron Block Slag Filling Technology for Localized Converter Repair

Common repair methods for large converters mainly include slag repair and material replenishment repair. However, excessive filling materials can increase refractory consumption and may introduce inclusions into molten steel, affecting steel cleanliness and slag removal efficiency.

To overcome these issues, iron block slag filling technology has been developed as an innovative converter repair method.

This technology utilizes rapid heat exchange and temperature gradients between iron blocks and high-temperature liquid slag to achieve rapid cooling, solidification, and bonding. Weak areas of the converter lining can therefore be repaired efficiently while reducing refractory material consumption.

Iron block slag filling is particularly suitable for repairing slag line areas and molten pool surfaces. During operation, slag basicity and composition are carefully controlled in the previous heat. Pre-prepared iron blocks weighing approximately 2–3 tons are evenly added into designated positions using a scrap charging hopper.

During the next heat, the iron blocks become fully immersed in the liquid slag. Rapid heat transfer between the iron blocks and high-temperature slag lowers slag temperature quickly, allowing the slag to solidify and adhere firmly to the furnace lining surface.

This process enables fast local repair of damaged lining areas while improving converter refractory maintenance efficiency and extending furnace campaign life.

Improved Converter Slag Retention Operation

In optimized converter slag retention practice, not all slag is poured out after slag splashing. Instead, part of the high-temperature, high-basicity slag containing a controlled amount of FeO is retained for the next heat.

This retained slag promotes rapid slag formation in the following heat, improves slagging efficiency, enhances thermal utilization, reduces slag-forming material consumption, and minimizes metal loss. More importantly, it helps reduce converter lining erosion.

With the continuous optimization of slag splashing technology and improvements in top-and-bottom combined blowing converters, steel plants have further refined slag retention practices to improve operational safety and refractory protection.

The converter final slag contains a certain amount of FeO. When retained slag contacts molten iron in the next heat, the following reactions occur:

(FeO)+[C]=[Fe]+CO

2(FeO)+[C]=2[Fe]+CO2

If the slag oxidation level is too high and FeO content exceeds 20%, both reactions may occur simultaneously, causing rapid gas generation and potentially resulting in dangerous slag splashing accidents.

Therefore, controlling gas accumulation and slowing reaction rates are critical. Since the carbon content in molten iron changes very little, controlling FeO content in the retained slag becomes the primary focus.

To ensure operational stability, two key measures are implemented:

  • Reduce final slag FeO content by optimizing blowing end-point control, carbon adjustment timing, and bottom stirring intensity.
  • Add 1000–1500 kg of lime before molten iron charging to dilute and cool the retained slag.

At the same time, the total slag amount in slag-retaining operations must be controlled to avoid excessive slag oxidation and unstable furnace temperatures. These measures effectively reduce reaction intensity, minimize splashing risks, and slow down converter lining wear.

Strengthening Daily Converter Refractory Management and Predictive Maintenance

In addition to process optimization, strengthening daily refractory inspection and predictive maintenance is equally important for extending converter campaign life.

Steel plants should establish a comprehensive monitoring system for key erosion areas such as the slag line, molten pool, trunnion zone, and tapping side. Regular inspection of refractory thickness, thermal conditions, and erosion patterns allows operators to identify abnormal wear early and take corrective measures before severe damage occurs.

Combining optimized furnace design, advanced slag splashing technology, iron block slag repair methods, and scientific slag retention practices with high-quality magnesia carbon bricks can significantly improve converter operational stability.

Modern converter maintenance technology not only reduces refractory consumption and maintenance costs but also improves steelmaking efficiency, production safety, and furnace campaign consistency. For steel plants aiming to reduce operating costs and improve productivity, comprehensive converter lining protection technology has become an essential solution for achieving long-term economic benefits.

FAQ

What causes converter lining erosion in steelmaking?

Converter lining erosion is mainly caused by high-temperature slag corrosion, thermal shock, chemical reactions, molten steel impact, and mechanical wear during oxygen blowing operations.

Why are magnesia carbon bricks widely used in converters?

Magnesia carbon bricks offer excellent slag resistance, thermal shock resistance, and high-temperature strength, making them ideal for converter refractory linings.

How can steel plants extend converter refractory life?

Steel plants can extend converter refractory life through optimized furnace design, improved slag control, regular maintenance, predictive monitoring, and advanced slag splashing practices.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information