Ladle lining can be divided into integral lining and brick lining. The former is mainly Al2O3 raw materials (natural sintered bauxite) and synthetic Al2O3 (white corundum, sub-white corundum and plate-like Al2O3, etc.) and is equipped with Sp, MgO, etc. to produce the so-called Al2O3-containing MgO low cement (LCC) or ultra-low cement (ULCC) refractory castables. In order to further improve the corrosion resistance, alkaline refractory castables have also been studied in recent years. Except for some special applications, alkaline refractory castables are still in the experimental research stage. Although the problems of MgO hydration, bonding system, residual shrinkage, etc. have been basically controlled, the problems of slag penetration, slag sticking, and structural spalling also limit the application of alkaline refractory castables in ladle. Brick lining is mainly built with neutral bricks (high alumina bricks, Al2O3-MgO-C bricks, etc.) and MgO-C bricks.
In the past, the refining ladle mainly used MgO-Cr2O3 bricks and high-alumina bricks as refractory materials for lining the slag line and low-corrosion area. Considering the requirements of environmental protection, now, except for the VOD ladle, all have been chromium-free, and MgO-C brick or MgO-CaO-C bricks are used as refractory materials for lining the slag line. Low-carbon MgO-C bricks are used for lining the slag line of the ladle for vacuum refining of molten steel (including refining low-carbon and super-carbon steel).

Whether to use MgO-C brick or MgO-CaO-C bricks for the slag line of the refining ladle is mainly determined by the type of refined steel, slag characteristics and operating conditions.
The research results show that in CaO-SiO2 slag (low-basicity slag), MgO-CaO-C bricks have a higher corrosion resistance. The reason is: when MgO-CaO particles contact CaO-SiO2 slag, fCaO dissolved from MgO-CaO sand particles will immediately react with slag components to generate high melting point and 2CaO•SiO2 and 3CaO•SiO2 solidified and densely accumulated on the surface, making the slag highly viscous and forming a solid protective layer on the surface of the brick, thereby improving the durability of the lining of MgO-CaO-C brick.
At the same time, in CaO-Al2O3 slag, the loss of MgO-CaO-C brick is serious, and increases with the increase of CaO in the brick. The reason is that fCaO dissolved from the brick will immediately dissolve in the CaO-Al2O3 slag to generate low melting point substances such as 12CaO•7Al2O3, which are discharged from the surface of the brick into the slag in a molten state, accelerating the dissolution of the brick into the slag. On the contrary, MgO-C bricks are easily corroded by CaO-SiO2 slag, but have high resistance to Ca0-Al2O3 slag.
Therefore, it is necessary to select refractory materials for the slag line of the refining ladle according to the specific refining conditions and slag characteristics.
The main damage mechanism of the MgO-C lining of the slag line of the refining ladle is the oxidation of C. In addition to the direct oxidation of C, it is mainly caused by the operating temperature (greater than 1650℃) and high-temperature decompression operation. This is especially true under high-temperature decompression conditions.