Damage mechanism of ladle air bricks
There are four main reasons for ladle air bricks damage: thermal stress, mechanical wear, mechanical stress, and chemical erosion.
In actual production, the ladle temperature is 1000℃, and the molten steel temperature reaches 1600℃. The temperature difference between the two when in contact will produce large thermal stress, which in turn causes a very large thermal shock. The ladle is in a repetitive working environment. The thermal stress caused by the frequent temperature changes of the air bricks when they are in contact with the molten steel and the ladle is one of the causes of the damage of the air bricks. The key factor for the thermal stress of the air bricks is the change in temperature, and there are differences in the temperature changes of different parts of the air bricks.
When the air bricks are subjected to strong thermal shock, the layered peeling near the working surface causes the air bricks to be damaged.
There are three main situations in which the vortex scours the air bricks:
(1) When the air bricks are higher than the base bricks, the main reason for the damage to the air bricks is that the molten steel in the ladle forms a vortex that produces a huge shear effect and scouring effect on the side of the air bricks. Therefore, the scouring force is one of the reasons for the great damage to the base bricks of the air bricks. In a normal working environment, the air base bricks are used only once, and the part above the base bricks will be scoured away after one use.
(2) When the air bricks are level with the base bricks, the base bricks protect the air bricks. The vortex formed by the molten steel first scours the base bricks, causing the shear force of the air bricks to decrease accordingly.
(3) When the air bricks are lower than the base bricks, cold steel is easily accumulated on the working surface during normal work. Since the viscosity of the remaining cold steel is relatively large, it has a certain obstruction to the blowing. Therefore, in order to meet the refining requirements, it is necessary to increase the blowing pressure. In this way, the scouring force of the air flow on the air bricks is correspondingly increased, and the shear and impact strength is large, making them more easily damaged.
During use, the working surface of the air bricks at the bottom of the ladle is in direct contact with the high-temperature molten steel. Under the condition of cyclic use, the temperature in the ladle is always in a state of change. The temperature difference will occur from high temperature to low temperature during the use of the refractory material at the bottom of the ladle. There is a difference in the expansion coefficient of the original layer and the metamorphic layer of the refractory material, which makes the air bricks subject to shear stress, resulting in transverse cracks in the air bricks and even fractures.
In the normal production process, the working layer of the air bricks is in contact with the slag and molten steel for a long time, and the slag continues to erode and penetrate into the air bricks. The oxides such as MnO, MgO, SiO2, FeO, Fe2O3 in the molten steel and slag react with the refractory materials in the air bricks, the physical erosion caused by the melting and peeling of the working layer of the air bricks by the molten steel, and the chemical erosion caused by the continuous penetration of the slag and molten steel into the air bricks during the smelting process are the main reasons for the damage of the air bricks.
Common damage conditions of air-permeable bricks
Breakage of air-permeable brick core
When the ladle is placed in the converter after hot repair, the temperature inside the ladle is about 900℃, and the final temperature of the converter is basically 1630℃. The temperature difference causes the rapid cooling and heating to cause the brick core of the air-permeable brick to peel, and the thickness of the peeling is generally 10-20mm. Moreover, after the brick core is peeled, the peeled part will not fall off due to the taper, which affects the air permeability of the molten steel in this ladle.
Breakage of air-permeable brick seat brick
The rapid cooling and heating caused by the temperature difference can also cause the seat brick of the air-permeable brick to break, and the height of the fault is 100-200mm. The brick core will also break due to the erosion of the molten steel without the protection of the seat brick. This kind of fault is extremely harmful, especially in the later period of the use of the air-permeable brick, because the remaining bricks are short, it is easy to cause the bottom of the ladle to leak steel.
Low strength and poor corrosion resistance
When using an oxygen gun to clean the air bricks for hot repair, the normal rate is 9-12mm/furnace. If the strength is not enough, the height of the brick core will drop significantly each time it is cleaned. The air bricks will not be used for the specified normal life and will be offline in advance, affecting the normal turnover of the ladle and causing instability in production.
Damage caused by erosion and erosion of molten steel
When inert gas is sprayed through the air bricks, the air flow will generate a certain impact force on the exposed air bricks around them. The high-speed flowing molten steel and the air flow interact to form a vortex. When the air bricks are higher than the air seat bricks, their protruding parts are eroded and sheared by the vortex to form an annular groove.
Damage caused by excessive oxygen burning
When the ladle is not back-casted in time after continuous casting, cold steel will form at the bottom of the ladle. It is necessary to use an oxygen gun to clean the air brick core with oxygen. Burning oxygen against the air brick core will cause faster damage.
The core of the air-permeable brick is burnt off-center
When cleaning the air-permeable brick, the oxygen gun is used to press against the brick core. At this time, the burning oxygen is concentrated at one point, which makes it easy for the brick core to burn off-center, causing the surface of the brick core to be not flat but inclined, with a height difference of more than 50mm. The air-permeable brick is not breathable when it is burnt off-center, and each cleaning will increase the degree of deviation, causing it to be offline early.
The back-blowing gas pressure is low
The back-blowing gas is nitrogen with a pressure of 0.5MPa, and the oxygen pressure of the oxygen gun is 0.8MPa. When cleaning with oxygen, the molten steel liquid will be blown into the slit of the air-permeable brick, and the slit will be blocked after cooling, causing poor air permeability. The burning of the air-permeable brick core will be aggravated when it is cleaned again by hot repair.
Corundum material around the air-permeable brick and bricks falling off the bottom of the bag
When laying the bottom of the bag, a corundum self-flowing material with a width of 50 to 100mm is poured around the air-permeable brick seat brick to protect the air-permeable seat brick. Due to the insufficient strength of the corundum self-flowing material or construction problems, the corundum material around the air-permeable brick base brick falls off, and the molten steel infiltrates and causes the air-permeable brick to break; or the bottom brick around the air-permeable brick breaks, and the infiltration of molten steel causes the surrounding corundum material and air-permeable brick to break.
Conclusion
Based on the above analysis of the causes of damage, we conclude that the damage of air-permeable bricks is not only related to the material, shape and structure of the refractory material itself, but also closely related to the use environment, operation and refining process. In terms of refractory materials, scholars at home and abroad are constantly conducting research and experiments, including selecting different additives, aggregates, micropowders, etc., so that the refractory material forms a solid solution phase under high temperature environment, increasing and improving the material’s thermal shock resistance, slag resistance, etc.