The service life of the lining is an important economic and technical indicator of electric arc furnace steelmaking, which directly affects the operation rate, power consumption and refractory material consumption of the electric arc furnace. Therefore, improving the service life of the electric arc furnace lining is of great significance to improving production and steelmaking operation rate.
Furnace type and refractory materials used in various parts
Angang 100t ultra-high power electric arc furnace (hereinafter referred to as Angang electric furnace) has an eccentric furnace bottom steel-making form. The furnace shell is split, and the upper furnace shell has a water-cooled plate frame structure; the lower furnace shell has a butterfly bottom with a vertical periphery, and the internal masonry refractory materials constitute the molten pool. The furnace shell is used as one for use and one for backup. After the service life of the furnace expires, the furnace shell is replaced as a whole and rebuilt offline for backup. The refractory materials used in the main parts of the furnace lining are shown in Table 1.
| Types | Mg0/% | Ca0/% | SiO₂/% | C/% | Volume density/(g.cm⁻³) | Compressive strength/MPa | Flexural strength/MPa | Use location |
| Magnesia carbon bricks | ≥76 | / | / | ≥14 | ≥2.9 | ≥35 | ≥88 | Furnace wall working layer |
| Ramming material | ≥78 | ≥13 | ≤0.6 | / | ≥3.0 | / | / | Furnace bottom, furnace slope working layer |
| Gunning material | ≥70 | ≥8 | ≤6 | / | ≥2.0 | / | / | Repair furnace wall damaged parts |
Erosion mechanism of refractory materials for furnace lining
The service life of the furnace lining in the first furnace campaign after the Angang electric furnace was renovated and resumed production was 300 furnaces, with an output of about 30,000 tons. During the operation of the furnace campaign, the furnace wall was repaired by wet gunning and the furnace slope was padded with magnesia sand ramming materials. The consumption of gunning materials was 1.7kg/t, the consumption of ramming materials was 2.3kg/t, and the cost of refractory materials was 45 yuan/t, which did not reach the ideal service life. The erosion of the refractory materials of the furnace lining off the line was dissected and measured, and the erosion of each part is shown in Table 2.
| Location | Original thickness mm | Residual thickness mm | Erosion thickness mm |
| Furnace bottom ramming material | 550 | 350 | 200 |
| Slag line at the electrode hot zone | 500 | 150 | 350 |
| Slag line in the furnace wall gun area | 450 | 100 | 350 |
| Other parts of the furnace wall | 450 | 240 | 210 |
| Furnace slope ramming material | Loss downshift 100 ~ 150mm, sintering layer thickness 200mm | ||
During use, the refractory materials of the furnace lining are subjected to the physical impact of scrap steel charge, the radiation and reflection of the electrode arc, and the chemical erosion of molten steel and slag. Especially at the steel-slag interface, the graphite on the working surface of the magnesia-carbon brick is oxidized by the physical penetration and chemical erosion of the highly oxidizing (FeO content 25% to 30%) slag, forming a loose decarburized structure. After repeated high-temperature oxidation, decarburization, and erosion, it is finally lost in the molten state and flaking state under heat and slag erosion. The lining of the hot zone of the electrode is subjected to high-temperature radiation of the arc, and the lining of the furnace wall cluster oxygen gun area is eroded by the local slag steel circulation, making the lining erosion and damage of these two areas more serious. The furnace bottom and furnace slope are knotted with magnesia sand ramming material. The early furnace masonry knotting is not dense and the furnace sintering is not good. The loose defects of the magnesia sand working layer, under the action of bottom blowing and stirring, the slag infiltrates and reacts with the magnesia sand to form iron-rich magnesia fumite, which reduces the melting point of the magnesia sand and accelerates the dissolution of the magnesia sand. At the same time, when the sintering is not sufficient in the early stage of the furnace service, it is subject to collision, vibration and impact of the charge, forming local pits at the bottom of the furnace, causing excessive corrosion in the local area.
Measures to improve the service life of the furnace lining
01 Strictly build the working layer of the furnace lining and tie it with the furnace bottom and furnace slope
The working layer of the furnace wall is made of dry magnesia carbon bricks, which are staggered and stacked. The brick joints should be less than 1mm. When building, it is necessary to prevent the impact from causing internal cracks, which will cause breakage and falling blocks during use, affecting the service life. The furnace bottom and the furnace slope working layer are tied with magnesia sand ramming materials. The first layer of magnesia sand is appropriately thick (about 40% of the total thickness). Use a compressed air vibration hammer to ram from the edge of the furnace in a circular manner to the center, and then ram from the center to the edge radially. Ram 3 times for each layer, so that the hammers are interlocked and the layers are connected and interlocked. The furnace slope is rammed with a compressed air vibration fork, which relies on vibration to fully expel the air in the magnesia sand ramming material, so that the ramming is smooth, dense, and strong in integrity. The inclination of the furnace slope is controlled to be <45° for later maintenance. When a new furnace is opened, a thin steel plate is used to cover the furnace bottom with a qualified lining to prevent the impact of the charging on the furnace bottom. At the same time, moisture-proof measures should be taken after the offline masonry is qualified.
02 Do a good job of baking and sintering the new furnace lining
A high-quality furnace lining should have sufficient strength after baking and sintering, and the entire furnace lining should be integrated. The first three furnaces of the new furnace are mainly baked linings, and all scrap steel smelting is implemented to prevent the impact of molten iron on the furnace lining. In principle, scrap steel is added in 2 to 3 batches, mainly light and thin materials, to reduce the impact of heavy materials on the furnace lining. Short arc and low power power supply are used, and the secondary voltage is controlled at 45 to 650V and the secondary current is controlled at 40 to 45KA. The furnace wall cluster oxygen gun uses the burner mode to blow oxygen to assist melting, and the oxygen flow rate of each gun is controlled below 750Nm³/hr to reduce the impact of high-speed cluster oxygen flow on the furnace bottom. After each batch of materials is melted through the well to form a molten pool, the power should be turned off and the furnace should be “braised” for 30 minutes. The temperature of the molten steel is used to ensure the low-temperature sintering and compact performance of the furnace lining.
03 Optimize the operation process to reduce the erosion of the furnace lining due to improper operation
Reasonable loading and distribution, use light and thin materials as the bottom, prevent the impact of heavy materials on the furnace bottom and furnace slope to produce pits, and accelerate the damage of refractory materials. After the basic molten pool is formed during the smelting and melting period, it is necessary to promptly spray or add carbon powder to the molten pool through the furnace wall carbon powder spray gun or the fourth feeding hole, switch the furnace wall cluster oxygen gun to the oxygen blowing mode, and adjust the oxygen flow ratio of the three furnace wall oxygen guns in time according to the situation in the furnace, so as to promote the C-O reaction to generate CO gas, increase the persistent foaming height of the molten pool slag, quickly realize the foam slag submerged arc operation, and reduce the arc light and high-temperature molten steel erosion of the furnace lining. At the end of smelting, as the C-O reaction weakens, the foam slag gradually becomes thinner. After the furnace door automatically flows slag, slag and lightly burned dolomite should be added in time to ensure that the slag basicity is always controlled at 2.0-2.5 and the original (MgO) content in the slag is 5%-8%, reducing the erosion rate of the furnace lining. Promote the operation of retaining steel and slag to ensure that 15-20t of steel is left in the furnace. After the steel is tapped, add 500kg of lime to thicken the remaining slag. While reducing the impact of charging on the furnace lining, it is also beneficial to make molten slag with a certain basicity in the next furnace early, reduce the reaction of free oxides such as SiO₂, P₂O5, Fe₂O₃ in the slag with MgO in the refractory, reduce the melting point of the refractory surface of the furnace lining, and aggravate the damage of the furnace lining.
04 Strengthen the maintenance of the furnace lining in the later stage
The maintenance of the main parts of the furnace lining in the later stage plays an important role in extending the service life. The lower area of the furnace wall oxygen gun and the “hot spot” area of the electrode should take enhanced gunning measures, make good use of the steel-out time and the temperature in the furnace for high-temperature fast repair and thin repair, and control the gunning thickness to 10-20mm to improve the adhesion rate of the gunning material and the rapid high-temperature sintering effect. In the later stage of use, pay attention to the erosion of the furnace slope, use ramming materials to fill the furnace slope in time, ensure that the angle of the furnace slope is always maintained at about 45°, and prevent the furnace slope from being severely deformed. At the same time, it is also necessary to prevent the furnace slope from rising due to improper padding, reducing the volume of the molten pool, increasing the molten steel surface, and affecting the stable and smooth operation.
The effect of improved use
During use, the life of the furnace lining is damaged by erosion due to mechanical action, high temperature action, chemical erosion and operating process. By improving the quality of furnace lining, improving the operation process and strengthening the maintenance of the later period of furnace service, the furnace life has been gradually increased from 300 furnaces to about 500 furnaces, and has remained stable. The cost of refractory materials per ton of steel has been reduced from 45 yuan to the current 22 yuan. The extension of furnace service life and stable use have improved the production operation rate, stabilized the production order, and achieved good results.