The function of a steel ladle in a steelmaking plant is to transport molten steel from the converter to continuous casting. On the ladle’s turret, molten steel at 1500℃ flows through the nozzle and slide gate at the bottom of the ladle into the tundish for billet transfer and pause. Finally, it flows from the tundish nozzle to the continuous casting leveling stage to complete billet forming. The nozzles from which the high-temperature molten steel flows out of the ladle need to be installed inside the nozzle seat bricks. During the ladle’s operation, the nozzles can be replaced online after 20-25 uses. The nozzle seat bricks must be replaced during minor ladle repairs, specifically when replacing the ladle bottom. The quality of the nozzle seat bricks and the quality of their installation directly affect the normal operation of the ladle. Common quality problems with ladle nozzle seat bricks during operation include unstable materials, problems with the bridging process control, inadequate baking, and defects in on-site construction and installation. This article reviews and resolves the problems encountered with the sprue bearing bricks on-site, ultimately achieving satisfactory results and ensuring the normal operation of the steel ladle.
01. On-site Situation of Steel Ladle Use
A steelmaking plant in a certain enterprise uses 150-ton steel ladles with double sprues. The sprues are directly embedded inside the bearing bricks, which are installed at the bottom of the ladle during the laying of the magnesia-carbon bricks. The bearing bricks have a lifespan synchronized with the ladle bottom, ranging from 70 to 80 heats. The overall lifespan of the steel ladle is between 130 and 150 heats.
The sprue bearings are installed after the ladle is baked and before it goes online. Sealing mortar is applied to the outside of the sprue, and the sprue is manually embedded into the bearing bricks using strong pressure. This ensures a tight connection between the bearing bricks, mortar, and sprue, increasing overall strength. During use, the top part of the sprue brick directly contacts the initial impact of molten steel. As the molten steel flows out, it is continuously eroded and washed away, causing the brick’s length to shorten. The nozzle inside the brick serves as the direct channel for molten steel flow, enduring the impact, friction, and temperature fluctuations of the high-temperature molten steel. Its connection to the brick relies on sealing mortar.
From July to September 2019, cracks appeared in the nozzle and sprue bricks. Timely repairs resulted in removal from the production line; delays led to steel leakage through the mortar channel between the nozzle and the brick, severely disrupting production, increasing ladle costs, and putting production in a passive position.
Regarding the steel leakage accident between the sprue and the nozzle caused by cracked sprue, an analysis and investigation were conducted from multiple aspects, including nozzle quality, composition, sprue quality, and construction. The nozzle was intact and undamaged, so the cause could be ruled out. The cracks found in the sprue were mainly due to the cracks in the sprue, which resulted in incomplete integrity and reduced strength. At the same time, the gap between the sprue and the nozzle increased, allowing molten steel to seep into the gaps in the sealant. The overall strength of the sprue, sealant, and nozzle, which form a unified structure, was compromised. The sealant could not withstand the high temperature of the molten steel and was gradually corroded, resulting in steel spitting and leakage accidents.
02. Solutions and Measures Taken for Steel Leakage
Regarding the steel leakage incident caused by cracks in the bedding bricks, the steelmaking plant and technical center personnel, in conjunction with the manufacturer, analyzed the cause. Firstly, the manufacturer analyzed and adjusted the bedding brick material. Secondly, products from other domestic bedding brick manufacturers with good quality and reputation were urgently sourced for trial use. The results are as follows:
1) Bedding bricks from manufacturer A were used on-site. After approximately 60 uses, micro-cracks were found, and the upper part of the bedding brick showed obvious diameter expansion.
2) Bedding bricks from manufacturer B were also found to have multiple longitudinal micro-cracks, distributed at 90-degree angles in the middle of the bedding brick (using the bedding brick as a horizontal reference from the ladle hot repair platform, the cracks were not at the four corners of the bedding brick).
3) The ladle contractor analyzed the material of the bedding bricks, selected high-quality raw materials, and gradually refined the formula. The formula and composition of the internal aggregates and powders were also adjusted. The results were summarized during use, and the probability of cracking gradually decreased.
03. The following measures were taken regarding the installation of the seat bricks
The seat bricks were laid together with the ladle base during installation. Before positioning the seat bricks, impurities were cleaned and filled at the steel structure location at the bottom of the seat bricks. The surrounding area was then vibrated and filled with castable refractory. After the overall construction was completed, the ladle was baked before being put into service.
1) The water-cement ratio of the castable refractory around the ladle seat bricks was strictly controlled, with the moisture content maintained between 6-8%.
2) Castable refractory construction: For the gap (30-100mm) between the seat bricks and the ladle base, manual operation was used during vibration; vibratory rods were not allowed to avoid excessive vibration force and aggregate settling.
3) When replacing the sprue online, the seat bricks were inspected for cracks and erosion.
4) Frequent communication with the dispatcher was maintained. If the waiting time for the ladle to come off the line exceeded 30 minutes, a second baking was performed.
5) Strict temperature monitoring is required during ladle baking. A dedicated logbook should be used to record the temperature of various parts (bottom, wall, slag line, and mouth). Close attention should be paid to the venting status at the ladle nozzle and on the ladle wall during baking.
6) The manufacturer, in conjunction with the company’s technical center personnel, will provide a complete on-site ladle construction plan, which will be displayed and regularly trained.
04. Results After the Modification
Through nearly two months of work on several aspects of the refractory bricks, the cracks gradually decreased and disappeared, and their service life remained within a controllable range. The modification was well-directed and effective, curbing production accidents and saving refractory material costs.
Steel ladles are crucial tools for transferring molten steel in steelmaking. The quality of the internal refractory materials and the quality of construction directly affect the smooth and safe operation of production. The daily management and allocation of ladles require exploration and summarization by technical personnel in each steel plant based on their specific operating conditions. The above experience is worth learning from and promoting.