The Causes of Slag Accretion in Steel Ladles

Severe slag accretion or “skulling” on ladle walls occurs during service, with the thickness of the accretion layer increasing as the number of heats progresses. This buildup reduces the effective volume of the ladle and increases its dead weight, which can easily reach or exceed the maximum crane hoisting capacity, posing significant safety risks to crane operations. Furthermore, it obstructs the smooth addition of alloys and drainage sand, hindering stable production. The removal of heavy slag buildup often damages the castable at the ladle mouth, leading to a reduced ladle service life, higher refractory consumption, and increased costs per ton of steel. Additionally, since the accretion layer is typically uneven and distributed irregularly, it complicates the accurate assessment of the residual lining thickness; incorrect judgments can lead to catastrophic breakouts.

Refractory Lining for Refining Ladle

Generally, ladles are designed with a monolithic lining, using alumina-magnesia (Al-Mg) castables for the working layer. New ladles do not typically exhibit slagging during the initial stage; however, accretion begins after approximately 5 heats and peaks in terms of weight between 30 and 40 heats. After repeated cycles, cracks develop in the castable, allowing molten steel and slag to penetrate and form a “sandwich” structure composed of layers of castable and cold steel. Overweight ladles exhibit not only thick wall accretion but also severe skulling at the ladle mouth. The accretion layer is often interleaved with cold steel, which reinforces the high-melting-point slag phases. This cold steel acts as an anchor for the slag layer. Therefore, the cracking of the castable during service combined with the anchoring effect of cold steel are the primary causes of severe ladle slag accretion.

Causes of Castable Cracking

The cracking of the castable is primarily attributed to the reaction between fused magnesia and fused corundum within the matrix during service. This reaction forms spinel, accompanied by a volume expansion of approximately 8%. This expansion induces cracking in the castable and degrades its resistance to slag penetration, ultimately leading to slag accretion during operation.

Analysis of Cold Steel Adhesion

The adhesion of cold steel is primarily caused by the poor thermal insulation of the ladle. Currently, only carbonized rice husk is used for insulation. However, its poor spreadability often results in heap-like formations rather than a rapid, uniform covering of the molten steel surface. Consequently, portions of the melt are frequently exposed to the atmosphere, accelerating heat transfer and negating the intended insulation effect.

Furthermore, the insulating performance of carbonized rice husk is suboptimal. While it acts as a heating agent after carbonization, its low calorific value and short chemical reaction duration prevent the formation of an effective thermal barrier. Significant heat loss persists throughout the process; by the middle and late stages of casting, the surface cover layer is often observed to be glowing red. This indicates rapid burn-off of the rice husk, which leaves the slag layer exposed and prone to cooling, eventually forming a slag crust that adheres to the ladle walls.

Measures to Prevent Ladle Slag Accretion

Enhancing the Slag Resistance of Ladle Castables

For slags with high iron oxide (FeO) content, the cement content in the castable is appropriately increased. The CaO within the cement reacts with corundum powder to form calcium hexaaluminate (CA₆), establishing a microstructural phase combination of magnesium-aluminate spinel (MA),CA₆,and alumina (A). This network structure mitigates the volume expansion associated with spinel formation, thereby reducing monolithic lining cracking and preventing slag accretion. Furthermore, while increasing the addition of fine magnesia powder improves erosion resistance, it negatively impacts slag penetration resistance. By balancing these properties, the magnesia fine powder content in the original formulation was optimized, being reduced from 6% to 4%.

Implementing Ladle Lidding for Thermal Insulation

A full lidding policy has been implemented for all ladles at the continuous caster. The ladle lids are connected to the ladles via a flexible hook system, ensuring they move in tandem as a single unit. This integrated design ensures that as soon as the ladle is hoisted to the caster, the lid remains in place to provide continuous thermal insulation.

Schematic of insulated ladle lid

 

Fig. 1 Schematic of insulated ladle lid

Utilizing On-line Rapid Ladle Heaters to Increase Empty Ladle Temperature

An on-line rapid ladle heater was installed at the post-furnace station, capable of raising the ladle temperature to 900℃ within 5 minutes. This significantly reduces the temperature drop of the molten steel, thereby minimizing slag and steel adhesion. Additionally, these heaters shorten the ladle turnover cycle and reduce the “black ladle” rate (the frequency of cold ladles). Through the high-efficiency modernization of the continuous casting machine, a better match between the furnace and the caster is achieved. This optimization has reduced the number of on-line ladles in service, consequently shortening the ladle turnover period.

Factors Affecting the Service Life of Refractory Linings in Refining Ladle

Impact of Ladle Brick Material

In the early stages of ladle furnace (LF) refining, conventional high-alumina and magnesia-alumina bricks were employed. These bricks experienced rapid erosion, originating at the slag line and quickly extending downward into the melt bath area, leading to slag-line breakouts and premature decommissioning of the entire ladle. By upgrading the material to magnesia-carbon (MgO-C) or magnesia-alumina-carbon (MgO-Al₂O₃-C) bricks, erosion in the melt bath working layer and the downward progression of the slag line were significantly decelerated. Although the slag line showed minimal downward shift after approximately 20 heats, severe localized erosion persisted. Analysis indicated that arc radiation and the turbulent scouring of the upper steel-slag layer increased the probability of spalling, causing instability in slag-line durability. By implementing tar-bonded improved MgO-C bricks at the slag line and optimizing slag fluidity, the service life of the slag line was synchronized with that of the melt bath working layer.

Impact of Lining Masonry Quality

Tracking of the ladle service process revealed that areas exhibiting severe “flame out” from brick joints during the preheating phase experienced the most intense erosion during operation. These joints are highly susceptible to steel leakage, primarily due to excessive joint width which facilitates the infiltration and corrosive attack of molten steel and slag.

Impact of Purging Plugs (Porous Plugs) on Service Life

  • Material Impact: Initially, corundum-based purging plugs were used. Due to suboptimal quality, these plugs frequently became clogged or completely blocked, necessitating forced replacements. This often resulted in leakages at the plug mounting site, negatively affecting the overall ladle life.
  • Positioning Impact: If the purging plug is installed too close to the ladle wall, the upward steel flow during argon stirring exerts a violent scouring effect on the adjacent lining. This accelerates brick erosion and significantly reduces the ladle’s service life.

Impact of Electric Arc Radiation

During the waiting period between primary furnace tapping and refining, carbonized rice husk is typically added for insulation, which often causes the slag to crust. In the early stages of refining, the arc remains exposed and cannot be submerged by the slag. Consequently, high-temperature arc radiation strikes the ladle wall directly, leading to localized overheating and structural damage.

Human and Operational Factors Affecting the Service Life of Refining Ladles

Impact of Improper Operational Management

  • Preheating of New Ladles: The service life of the lining is closely related to the quality of the initial preheating process. Since the ladle uses magnesia-carbon (MgO-C) or magnesia-alumina-carbon (MgO-Al₂O₃-C) bricks, inadequate preheating causes a rapid temperature spike during initial service. This triggers the violent escape of gases (water vapor and tar pyrolysis gases), leading to severe erosion at the joints. This is a primary cause for the formation of deep pits or cavities along the brick joints.
  • Cold-Ladle Tapping and Steel Washing: Tapping into a cold ladle subjects the lining to thermal shock from rapid heating and cooling, resulting in intense erosion. Furthermore, cold-ladle tapping causes a significant temperature drop in the molten steel, necessitating longer refining times and thus exacerbating the erosion of the lining and slag line. When ladle turnover is tight and preheating is bypassed or insufficient, the practice of “washing the ladle” with molten steel often leads to cracking or spalling of the bricks, significantly shortening the ladle’s life.
  • Improper Argon Stirring: Leakages at the argon pipe connections, poor permeability of the purging plugs, or a mismatch between the argon flow rate and power input can result in large vertical temperature gradients. This leads to excessive temperatures at the slag line and upper melt bath, causing severe localized lining erosion.

Impact of Improper Primary Furnace Tapping

  • Unstable Tapping Volume: Fluctuations in tapping volume lead to severe erosion of the non-slag-line lining. In particular, when the tapping volume is low, the slag line shifts downward onto the melt bath working face, which has a more detrimental impact on the overall service life.
  • Unstable Tapping Temperature: Low-temperature tapping extends the required refining time, which further intensifies the thermal and chemical attack on the ladle lining.
  • Slag Carry-over during Tapping: Frequent slag carry-over from the primary furnace introduces highly oxidative slag that reacts with the lining, especially at the slag line. This reaction forms low-melting-point substances, leading to the erosion of the reaction layer. Additionally, excessive oxidative slag prolongs the refining process, causing severe degradation of the slag line and lining.

How to Improve Masonry Practices to Extend the Service Life of LF Refining Ladles?

Optimization of Ladle Masonry Processes

  • Material Optimization: For the melt bath working layer of refining ladles, magnesia-carbon (MgO-C) or high-quality magnesia-alumina-carbon (MgO-Al₂O₃-C) bricks must be utilized. For the slag line, high-grade MgO-C bricks with appropriate antioxidants should be implemented. On the slag-dumping side, approximately 10 high-quality MgO-C bricks should be integrated into the center of the first and second layers. Furthermore, the gap between the permanent layer and the working layer should be tightly packed with a few millimeters of magnesia sand.
  • Enhancing Masonry Quality: The construction quality of the working layer must be strictly controlled to ensure that brick joints are less than 1 mm and the height variance between bricks in the same layer does not exceed 1.5 mm. Staggered joints between adjacent layers are mandatory. During the installation of purging plugs, they should be repositioned toward the center of the ladle. Joint widths between the bottom bricks and the purging plug blocks must be less than 2 mm to mitigate the erosive scouring of the adjacent lining by the steel flow.

Improvement of Ladle Bottom Masonry

During EBT (Eccentric Bottom Tapping), the molten steel directly impacts the ladle bottom. To counter this, the thickness of the refractory bricks in the impact zone has been increased, with the MgO-C bricks being 50 mm higher than the surrounding area and upgraded to 18A grade, effectively extending the bottom’s service life. Previously, intermediate maintenance (mid-life repair) focused on replacing the nozzle and purging plug well blocks without a full bottom overhaul, using alumina-magnesia spinel castables to patch the surrounding areas. However, deep pits often formed after 5–6 heats, necessitating wet patching to prevent severe steel contamination and increased inclusions.

The current practice minimizes the volume of castables used during mid-life repairs, instead utilizing vibration rods to compact the poured castable, which has yielded superior results. The leveling and filling of the nozzle and purging plug well blocks must strictly adhere to technical operating procedures. Specifically, the brine concentration must be maintained above 1.3 mol/L to ensure the proper sintering of magnesia powder. Failure to do so allows unsintered powder to leak through joints due to ladle vibration and rotation, creating voids that can lead to cracks and subsequent steel penetration under high ferrostatic pressure.

How to Improve Ladle Structure to Extend the Service Life of LF Refining Ladles?

Addition of an Insulation Layer

To enhance thermal retention, an insulation layer (insulating board) was added between the permanent layer and the ladle shell. Under typical conditions, this reduces the temperature drop of the molten steel during casting from the original rate to a significantly lower level. When combined with tundish lidding, the temperature fluctuations during the early and late stages of casting can be maintained within a range of 12℃. This technology addresses the poor thermal insulation of the permanent layer, enabling lower tapping temperatures, shorter refining times, and reduced power consumption, while simultaneously mitigating the erosive scouring of the MgO-C working layer by high-temperature steel.

Optimization of the Permanent Layer

Due to prolonged refining times and harsh operating conditions, refining ladles typically suffer from low service lives. The permanent layer was upgraded from a brick-masonry structure to a monolithic casting. The original permanent layer, constructed with thin clay bricks and high-alumina mortar, was prone to breakouts whenever steel penetrated the MgO-C joints of the working layer. The improved permanent layer utilizes alumina-magnesia spinel castables formed through one-time integral casting. This creates a smooth, gap-free internal surface resistant to slumping or spalling after air-drying and preheating. This transition has fundamentally controlled breakout accidents caused by joint penetration, thereby extending ladle life and ensuring safe, stable production.

Treatment of “Steps” Between New and Old Refractories During Mid-life Repairs

During mid-life repairs, a “step” of 20–60 mm typically forms at the interface between new and old magnesia-carbon bricks. If left untreated, the argon-stirred molten steel creates vortices at this junction, turning it into a structural weak point. Consequently, after replacing the slag line, this area is leveled using a MgO-C based mortar mixed with resin. Since the mortar’s composition closely matches that of the MgO-C bricks and the resin provides excellent adhesion, the interface problem is effectively resolved. This treatment is particularly effective during the mid-to-late stages of a ladle’s campaign or under emergency conditions (e.g., severe slag-line erosion) when the remaining wall thickness is between 80–100 mm.

Handling of the junction step in mid-campaign ladle repair

 

Fig.2 Handling of the junction step in mid-campaign ladle repair

Improvement of Mortar Quality

Utilizing MgO-C based mortar for masonry, which shares nearly identical chemical and physical properties with MgO-C bricks, addresses the following issues:

  • Joint Leakage: Prevents “run-out” through brick joints.
  • Erosion Reduction: Minimizes localized scouring at the joints.
  • Maintenance Efficiency: Since this mortar does not bond with the permanent layer (Al-Mg spinel), the labor intensity for de-lining is greatly reduced. It also maintains a smooth permanent layer surface, providing a superior foundation for high-quality re-masonry.

Furthermore, the application of MgO-C mortar for repairing cracks and cavities in cooled ladles has proven highly effective. These weak points are significantly reinforced, with no issues detected after a full service cycle. The performance is markedly superior to the traditional method of using magnesia powder mixed with brine.

Extending Refining Ladle Life through Enhanced Preheating and Operational Maintenance

Strict Operational Management of Refining Ladles

The quality of ladle preheating must be strictly controlled; new ladles must be preheated for at least 8 hours (until reaching a “red-hot” state), and the practice of “washing” cold ladles with molten steel is strictly prohibited. Before each heat, the argon system must be tested to ensure no leakages in the piping. Connections at the bottom of new ladles must be sealed with copper or steel gaskets to ensure the integrity of the purging plug and the application of appropriate stirring pressures.

Operational accidents represent the most significant source of waste. Steel penetration through the upper nozzle or sliding gate results in metal loss and damage to the ladle shell, which severely disrupts normal operations and may even necessitate premature decommissioning and complete de-lining. Furthermore, poor or failed permeability of the purging plug leads to localized overheating of the slag and upper steel during refining, causing intense erosion of the MgO-C bricks at the slag line. Other incidents, such as slag-line leakages or brick spalling, cause abnormal ladle turnover and lead to the hydration/pulverization of the refractory lining, ultimately reducing service life.

Therefore, technical preparation protocols must be rigorously enforced through strict assessment and management. Enhancing preheating quality and ensuring ladles are commissioned in a red-hot state minimizes the thermal shock exerted by high-temperature molten steel on the refractory bricks. The first three heats of a new ladle are critical; continuous operation is required to ensure proper sintering of the MgO-C bricks, thereby enhancing their refractoriness.

In-service Maintenance and Repair

During the service cycle, weak points such as pits, cavities, or cracks often develop at the slag line, well blocks, and impact zones. These can be addressed using hot-patching materials, which typically allow for an additional 4 to 6 heats of continuous use. Given the harsh working environment and operational difficulties for workers, shotcreting (spray repair) is an effective alternative. The MgO-C based hot-patching material is a dry-type mix that typically requires only 20 minutes of sintering in a red-hot ladle before returning to service.

How to Optimize Operations to Extend the Service Life of LF Refining Ladles?

Rational Management of Ladle Turnover

As a critical link between processes, the ladle is essential for smooth production flow; conversely, production disruptions negatively impact ladle life. For instance, during operational incidents, a ladle may remain in a refining or standby state for up to 10 hours. Therefore, the deployment of older ladles must be strategically coordinated. Due to current imbalances in the EAF-LF-CC (Continuous Casting) process matching, the first heat of a sequence often requires prolonged refining times and higher tapping temperatures. Consequently, older ladles should avoid the first heat whenever possible to effectively extend their service life and minimize the risk of accidents.

Strengthening Furnace-Front Operations

Effective control of hazardous factors is necessary to prevent the following scenarios:

  • Oxidative Slag Carry-over: If oxidative slag enters the ladle, it hinders the rapid formation of a reducing atmosphere and causes severe erosion of the ladle slag line.
  • Improper Slag Fluidity Control: Excessive use of fluorspar (CaF2) to adjust refining slag fluidity should be avoided. Overly fluid (thin) slag leads to intense scouring and erosion of the slag line area.
  • Excessive Tapping Volume: Beyond complicating the refining process and resulting in insufficient slag volume, overfilling directly threatens the slag line. The combined effects of argon stirring, electrode arc radiation, and molten steel buoyancy act directly on the top three layers of bricks, causing loosening, damage, or even spalling of the slag line bricks, which can lead to premature decommissioning.
  • Misalignment at the Refining Station: When a loaded ladle is placed at the refining position, it must be perfectly centered. Misalignment subjects the ladle to severe damage from electrode arc radiation. The No. 2 electrode area is a particularly high-temperature zone where accidents are most likely to occur.

How to Extend the Service Life of Steel Ladles?

Smelting Operations

  • Optimal Tapping Temperature Control: Excessive tapping temperatures cause severe erosion of the internal working layer. Conversely, temperatures that are too low extend the refining duration and the residence time of molten steel, leading to intense chemical erosion and mechanical damage.
  • Appropriate Iron Oxide (FeO) Content: High FeO concentrations trigger violent chemical reactions with the refractory lining, resulting in rapid erosive loss.
  • Maintenance of Proper Slag Basicity: Lower slag basicity correlates with more aggressive chemical attack on the ladle’s working layer.

Casting Operations

  • Vibration Control: Avoid violent vibrations that can lead to loosened bricks, widened joints, and the dislodgement of refractory mortar.
  • Thermal Shock Mitigation: Avoid rapid heating and cooling cycles or the use of water for forced cooling, which cause cracking and spalling of the lining bricks.
  • Strict Preheating Protocols: Rigorously execute the preheating schedule to ensure adequate ladle temperature and alleviate thermal shock during tapping.
  • Time Management: Prevent delays and prolonged residence times of molten steel within the ladle.

Masonry Quality

  • Guaranteed Construction Standards: Ensure high-quality masonry and precise joint control.
  • Material and Thickness Optimization: Select appropriate refractory materials and lining thicknesses tailored to the specific requirements of different ladle zones.
  • Monolithic Formation: Adopt monolithic lining technologies (such as integral casting or ramming) to eliminate joints.

Maintenance and Repair

  • Targeted Repairs: Perform timely maintenance on damaged sections of the lining.
  • Thorough Cleaning: Ensure the complete removal of residual slag and steel (skulls).
  • Patching and Coating: Fill and smooth out gaps or pits caused by steel scouring or mechanical damage using specialized mortars or coatings.
  • Hot and Cold Spray Repair (Shotcreting): Utilize both hot and cold spray repair techniques to reinforce weak areas and extend the campaign life.

Factors Affecting the Service Life of Steel Ladles

  1. Ladle Dimensions, Shape, and Configuration: Including the geometric design and structural integrity of the ladle.
  2. Process Conditions: Such as tapping parameters, ladle turnover rate, slag chemistry, electric arc heating (refining), alloying practices, and degassing processes.
  3. Ladle Operational Practices: The specific handling and management methods used during service.
  4. Refractory Types and Lining Design: The selection of refractory materials and the engineering design of the lining layers.
  5. Masonry Practices, Cleaning, and Maintenance: The quality of refractory construction, as well as the procedures for cleaning residual slag/steel and performing lining repairs.

Internal Factors Leading to High Erosion Rates of Ladle Linings

  1. Thermal Cycling: Even with the use of ladles and ladle lids, the thermal cycling associated with secondary steelmaking remains substantial. Consequently, refractory consumption is inherently higher than that in primary steelmaking furnaces.
  2. Thermo-mechanical Cracking: During the movement and hoisting of the ladle, thermo-mechanical cracks tend to develop within the thin refractory working lining.
  3. Thermal Gradients and Loss: High tapping temperatures and the intensified heat loss associated with certain types of stirring (e.g., gas or electromagnetic stirring).
  4. Chemical Erosion: Severe erosion of the refractory lining caused by superheated slag containing lime, calcium aluminate, and fluorspar  (CaF2).
  5. Lack of Protection: A typical lack of a protective slag coating or a spray-repair (gunning) layer, which are measures commonly used to extend the campaign life of primary steelmaking furnaces.

Primary Causes of MgO-C Brick Degradation at the Refining Ladle Slag Line

  1. Decarburization via Oxidation: The loss of carbon content due to oxidative reactions.
  2. Slag Infiltration: The penetration of molten slag into the decarburized layer.
  3. Chemical Reaction: The reaction between slag components and the MgO in the MgO-C bricks, which forms low-melting-point substances, resulting in the erosive loss of the reaction layer.
  4. Structural Deterioration: Oxidation or expansion of metallic antioxidants (additives), leading to tissue degradation and a loosened structure under intermittent operating conditions.
  5. Mechanical Failure: Cracking and spalling (shedding) caused by the insufficient strength of MgO-C bricks at elevated temperatures.

Reactions between fused magnesia and corundum form spinel with 8% volume expansion, inducing cracks that allow slag and steel to penetrate, leading to severe buildup and reduced volume.

MgO-C bricks offer superior resistance to arc radiation and turbulent slag scouring, especially when optimized with tar-bonding and antioxidants to synchronize wear with the melt bath.

Degradation occurs through decarburization via oxidation, slag infiltration into the decarburized layer, and chemical reactions forming low-melting-point substances.

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information