How to deal with the burnout accident of the blast furnace
The burnout accident of the blast furnace bottom is the most direct factor affecting the longevity of the blast furnace. We have conducted in-depth discussions on the causes of the burnout of the blast furnace hearth and bottom and the causes of the erosion of its carbon bricks in previous articles. So when the accident really happens, how should we deal with it and how to prevent it?

Treatment of burnout of the blast furnace bottom
The burnout of the furnace bottom is a very dangerous production safety accident. It will induce an explosion accident and cause a greater disaster, especially for water-cooled furnace bottoms. The burnout accidents of the furnace bottom that have occurred in history have all occurred in blast furnaces with small volumes, no cooling of the furnace bottom or air cooling of the furnace bottom. When the furnace bottom is burned through, the molten iron flows out from the air cooling pipe. Because there is no water accumulation around the furnace base, no more serious explosion accidents are induced. For blast furnaces with water-cooled furnace bottoms, we should always be vigilant. Once the temperature of the carbon bricks on the water cooling pipe exceeds the standard, the furnace should be stopped for overhaul as soon as possible to prevent the furnace bottom from burning through. There is no other way after the furnace bottom is burned through, and it can only be overhauled after the furnace is cooled.
Treatment of burnt-through furnace cylinder
The treatment of burnt-through furnace cylinder should first confirm whether the burnt-through part is above the full carbon bricks at the bottom of the furnace. If the burnt-through position is very low, above 1 to 2 layers of carbon bricks at the bottom of the furnace, emergency repair is meaningless. When the burnt-through part of the furnace cylinder is above the plane of full carbon bricks, it is necessary to determine whether there is still liquid iron in the furnace cylinder to prevent residual iron from flowing out when the furnace shell is opened to take the cooling wall and causing safety accidents. If the blast furnace has been in production for many years and is approaching the overhaul period, it is not economical to repair and resume production. It is best to quickly dismantle the furnace for overhaul.
Emergency repair of burnt-through furnace cylinder generally adopts the method of digging and patching. Under the condition that no liquid iron flows out when the hole is confirmed (if there is liquid iron, residual iron should be removed first), prepare carbon bricks (microporous small carbon bricks are best) and new cooling wall, cut the furnace shell and damaged cooling wall, support the carbon bricks above the burnt-through mouth, remove the residue and find the original brick surface, lay new bricks, install the new cooling wall, weld the furnace shell, press carbonaceous mud, and pass water through the cooling wall for leak test. If there are other damaged parts, they should be repaired and then resumed. The re-airing operation can be handled in the same way as the furnace freezing accident. The tuyere above the burnt-through part can be blocked for a long time according to the situation, and other furnace protection measures can be used to gradually resume production. The smelting intensity after resumption of production should be lower than the production level before the accident, and preparations for the overhaul of the next generation of furnaces should be made as soon as possible.
Prevention of furnace bottom burn-through
Preventing the occurrence of furnace bottom burn-through accidents is a system engineering with a wide range of aspects. In the first generation of blast furnaces, from the selection of blast furnace design schemes, design, manufacturing, construction, furnace opening, operation, production management, maintenance, supporting projects, etc., a series of links should be advanced and reliable to achieve real longevity. If any link fails to meet the requirements, it may cause the failure of the entire system, and finally manifest as failure to achieve the longevity goal.
Clues of furnace bottom danger should be discovered as early as possible, and corresponding measures should be taken to prevent the furnace bottom from burning through. There will be precursors to dangerous situations in blast furnaces. If there are no signs, it may be ignored due to lack of detection means, failure of detection means, and the appearance of dangerous signals. During the production period of the first generation of the blast furnace after it is put into operation, it is necessary to observe carefully and remain vigilant at all times. The following is an example to illustrate this.
Case Analysis
A certain enterprise has two 4000m3 blast furnaces. After overhaul and commissioning, they were in production for 3-4 years. In May 2008, the temperature of the carbon bricks at the bottom of the furnace reached 600℃. The following emergency measures were immediately taken:
(1) Reduce the smelting intensity and reduce the temperature in the short term
(2) Use vanadium-titanium ore to protect the furnace;
(3) Increase the amount of cooling water in the furnace from 2700m3/h to 4700m3/h;
(4) Strengthen the maintenance of the iron mouth and keep the iron mouth deep enough;
(5) Perform grouting treatment on the part of the furnace.
After taking these measures, after about two and a half years of repeated furnace protection, the blast furnace of the plant has basically achieved stable production since September 2010.
The following requirements are particularly important for the longevity of a newly commissioned blast furnace:
(1) The newly commissioned blast furnace should not overemphasize the speed of reaching full production. It is advisable to smelt cast iron in 10-20 days. This can generate a layer of graphite carbon in the furnace from the beginning to seal some brick seams, which is beneficial to prolonging the life of the furnace.
(2) While ensuring sufficient cooling water, close attention should be paid to whether there is any leakage in the cooling equipment, especially leakage in the tuyere and cooling wall.
(3) It is recommended to carry out vanadium-titanium ore protection for the new blast furnace once every six months after the start of the furnace, and once a year thereafter, to ensure that the temperature of the blast furnace carbon bricks and the temperature difference of the water are within the control range.
(4) Insist that the harmful elements contained in the raw materials and fuels entering the furnace during the first generation of furnace service are within the requirements specified in the regulations, and it is prohibited to enter the furnace in excess of the standard. For the harmful elements that are accumulated in the circulation, regular elimination measures should be taken.
(5) It is necessary to ensure that the iron mouth has sufficient depth for a long time.