Through the joint efforts of generations of ironworkers, my country has developed a relatively complete and stable production technology for long-life blast furnaces, achieving a balance between high efficiency and longevity. This includes advanced cooling technology, a well-designed furnace body structure, and high-quality refractory materials.
01 Extending the Service Life of the Lower Blast Furnace Body
Long-term research and practice in blast furnace production has led to the conclusion that establishing a non-overheating cooling system under high-intensity environments is extremely important for the lifespan of blast furnaces. A non-overheating cooling system refers to maintaining the cooling facilities at temperatures below the equipment’s upper limit under current smelting intensity conditions.
Before the 1980s, my country’s blast furnaces used ordinary ash cooling walls and open-loop industrial water circulation as cooling systems, neither of which could achieve a non-overheating state. Until the end of the 20th century, most of my country’s blast furnaces used ductile iron cooling walls, high-quality refractory materials, and closed-loop soft water circulation cooling systems in the lower part of the furnace body, effectively increasing the furnace body’s service life, but still failing to achieve a non-overheating state. Because the main material of ductile iron cooling walls has a low thermal conductivity, the anti-carburizing coating on the water pipe surface is prone to developing air gaps, leading to increased thermal resistance of the entire cooling wall. This ultimately results in higher temperatures in the blast furnace operating environment. Since the successful trial of copper cooling walls by MAN GHH in Hamborn No. 4 blast furnace in Germany from 1979 to 1988, the characteristic of copper cooling walls to maintain a non-overheated state under high-intensity smelting environments has been widely accepted. It possesses the following thermal characteristics:
① Low thermal resistance. Copper has highly efficient heat conduction capabilities and exhibits air gap-free thermal resistance. Its normal operating temperature is around 60℃. During normal production, the high-temperature liquid slag is cooled and hardened on the copper cooling wall surface, forming a hard slag shell that isolates the cooling wall from the high-temperature liquid slag, preventing slag erosion.
② Stable slag shell. Once slag shell peels off, a new slag shell quickly forms on the hot surface for protection. Test data shows that it takes approximately 15-20 minutes for a complete slag shell to form on the copper cooling wall surface.
Since 2000, copper cooling walls have been applied to the belly, waist, and lower part of the blast furnace. Through continuous experience accumulation, the blast furnace cooling system has been improved, resulting in a thin-walled blast furnace structure. The thin-walled blast furnace not only significantly increases the service life of the furnace body but also reduces the use of high-quality refractory materials during the design process, allowing for rapid production ramp-up after commissioning and maintaining optimal operating parameters for an extended period, thus achieving both high efficiency and longevity.
Based on recent practical experience in my country, the following issues still require attention:
① The design concept should be changed. Traditional cast iron cooling walls require protection with high-quality refractory materials. With the application of copper cooling wall technology, this is no longer necessary. As long as the cooling intensity is sufficient, the furnace body’s lifespan can be naturally extended, and the copper cooling wall can also avoid burn-out.
② The internal structure of the blast furnace needs further improvement. Since the promotion of copper cooling walls in key areas of the blast furnace, a new concept has emerged in the design of the internal heat-resistant structure: the long-term stable operation of the furnace body does not depend on refractory materials but on the stable operation of the cooling equipment.
③ The problem of slag shedding from copper cooling walls warrants further study. Extensive production data demonstrates the high stability of copper cooling walls. However, a problem exists: the slag forming on the dovetail grooves of the copper cooling walls located in the furnace waist and lower part of the furnace body is unstable. This means that setting up the dovetail grooves is not only wasteful but also fails to achieve the designed effect.
In actual production, slag shedding not only leads to intense heat exchange and significant heat loss but also causes rapid heat transfer within the copper cooling wall itself, resulting in irreversible plastic deformation. Although the change in shape is small, frequent slag shedding accumulates and leads to significant changes in shape, subsequently affecting production. Therefore, avoiding frequent slag shedding is a topic that requires in-depth research.
02 Design for Extending the Lifespan of the Hearth and Hearth Sections
The design of the blast furnace hearth and hearth sections was based on the following principles: Currently, the main cause of damage to the blast furnace hearth and hearth sections is the erosion and washing away by molten iron. To maintain the longevity of this area, a combination of high-quality carbon bricks and an efficient cooling system is necessary. This design concept has yielded excellent results.
The cooling system and carbon bricks must be effectively integrated. First, if the hearth section is not lined with carbon bricks, the cooling wall and the high-temperature molten iron inside the hearth will be in close contact, significantly increasing the heat load it needs to withstand. Second, even with the best carbon bricks, without a good cooling system, it is impossible to maintain the blast furnace hearth in good working condition for an extended period.
Improving the hearth cooling performance aims to push the 1150℃ (molten iron solidification temperature) isotherm as far into the furnace as possible. Throughout the entire production process of a blast furnace, the general concept of mutual dependence and coexistence between cooling and carbon bricks can be roughly divided into the following stages:
① Carbon brick erosion stage: In the early stage of blast furnace commissioning, regardless of the cooling method, since the carbon bricks on the hearth sidewall are initially relatively thick and have high thermal resistance, the 1150℃ isotherm will still remain inside the carbon bricks. At this stage, due to the constant erosion and scouring of molten iron, the carbon bricks are continuously corroded. The rate of erosion is related to their own mass, so the cooling method has little impact on the erosion of the carbon bricks at this time.
② Relatively stable stage: In the later stages of blast furnace operation, after long-term erosion, the carbon bricks accumulate to a certain residual thickness, and their thermal resistance decreases. At this time, a better cooling system can promote the 1150℃ isotherm to move away from the carbon bricks and into the furnace, resulting in the formation of a slag-iron solidification layer. This effectively slows down the erosion of the carbon bricks. Therefore, the stability of the hearth operation during this period mainly depends on cooling. Higher cooling intensity is more conducive to the formation of the slag-iron solidification layer.
③ Critical operating stage: In this stage, the remaining carbon bricks become very thin, which is reflected by the heat flux intensity value. The operating time of some blast furnaces indicates that when using cooling walls to cool the hearth, the heat flux intensity needs to be controlled at <10000W/㎡. A red warning is required when the heat flux intensity is ≥13956W/㎡ (12000KW/㎡·h), and the furnace hearth will burn through when the heat flux intensity is between 18000 and 21000W/㎡ (15477~18056KW/㎡·h).
03. Enhancing Awareness of Research on Hearth and Bottom Structures
① How to Understand High-Quality Carbon Brick Standards?
In recent years, using heat transfer theory as the design guide for important parts such as blast furnaces and hearths has been a significant advancement. However, excessive focus on the thermal conductivity of carbon bricks while neglecting their resistance to molten iron erosion is also undesirable. From a purely heat transfer perspective, this approach may seem reasonable, but four years of production practice have proven it to be unreasonable, ultimately leading to hearth burn-through.
② What is Good Cooling?
Good cooling ensures a uniform distribution of the 1150℃ isotherm from the hearth inner wall to the furnace interior. Domestically, there is consensus that the cooling intensity of the hearth should be increased. However, some believe that cast iron cooling walls are sufficient for the normal cooling effect of the hearth during use, while others insist that copper cooling walls are necessary in the taphole area and the “elephant’s foot” erosion area to ensure the hearth has the same lifespan as the furnace body. Further summarization and consensus are needed in future practice.