lmm@magnesiacarbonbricklmm.com

Technical support and construction service team

Improvement of slag splashing protection technology and furnace type control in converter steelmaking

Abstract: This paper introduces the improvement of slag splashing protection technology and furnace type control in steelmaking plants. By adjusting the final slag composition and basicity, the large surface of the converter is supplemented with iron blocks, and the steel tapping side (small surface) is filled with steel bar cut ends. After the molten slag after steel tapping is added with pig iron blocks and steel bar cut ends, it is naturally cooled for 3 to 5 minutes before slag splashing, which effectively improves the converter capacity and operation rate, reduces the cost of refractory materials, and increases the life of the converter.

Keywords: slag splashing protection: basicity; iron block; steel bar cut ends

1. Introduction

In recent years, the average steel consumption of a steelmaking plant has been stable at 695-730Kg/t steel. Because the iron consumption is low, the final molten steel is highly oxidizable, and the smelting rhythm is fast, it is crucial for the maintenance of the converter furnace condition. The two converters of the steelmaking plant adopt slag splashing protection technology, but the large and small surfaces of the converter need to be supplemented with supplementary materials, and the supplementary time is long, which limits the further improvement of production efficiency. For this reason, the steel mill has explored an effective method from the process. By controlling the end slag composition and basicity, according to the fluidity of the end slag, 1.5-2t pig iron blocks are added, and then the slag is splashed to quickly fill the large surface after cooling; because the production rhythm is fast, the proportion of steel tapping in the front furnace is high, and the maintenance of the small surface on the tapping side has always been carried out by replenishing the furnace charge + self-flowing material filling, which affects the improvement of the production rhythm. Now, after the steel is tapped, 1.5-2t of pre-prepared steel bar heads are added through a self-made feeding pipe after the furnace, and the slag is splashed after cooling for 3-5 minutes. The effect is very obvious, reducing the converter filling time from the original 45min to the current 5-8min. The operation rate of the converter has been greatly improved, the output of the converter has been greatly increased compared with the original, and the cost of refractory materials has also been greatly reduced.

2. Process equipment and parameters

The steel mill currently has two 80t converters, one 5-machine 5-strand and one 6-machine 6-strand 150×150mm small square billet continuous casting machine, mainly producing Q195 and Q235 steel grades. The continuous casting adopts liquid level automatic control technology, hydraulic shear cutting technology and hot charging and hot delivery technology, which effectively ensures the casting quality.

slag splashing

3. Slag splashing furnace protection technology

The four-step control method of slag splashing furnace protection refers to “slag making – slag adjustment – slag splashing – solid slag”. Slag making refers to controlling the FeO and MgO content in the slag reasonably to make sticky slag and reduce its erosion on the furnace lining. Slag adjustment refers to adjusting the slag to a state that is conducive to slag splashing at the end of smelting. Slag splashing refers to reasonably controlling the position of the slag splashing gun according to the erosion of the furnace lining to achieve the purpose of uniform slag splashing. Solid slag refers to improving the strength and corrosion resistance of the slag splashing layer.

Slag solidification operation steps: After slag splashing, although the slag splashing layer is formed, the temperature in the furnace is still high and the slag splashing layer has low strength. In order to improve the strength, cooling is the most effective method. Slag solidification operation is the process of cooling and sintering the slag splashing layer, which plays a role in improving the strength of the slag splashing layer.

Step 1: After the slag splashing is finished, the oxygen lance should be added to continue blowing nitrogen for cooling operation, that is, after the slag splashing is finished, the nitrogen is not turned off, and the oxygen lance moves up and down in the furnace at least twice to reduce the temperature of the slag splashing layer and increase the strength of the slag splashing layer. This step can be omitted for the furnace without slag adjustment.

Step 2: After the slag splashing operation is finished and the slag is poured, when preparing for the next furnace smelting, the operation sequence of adding scrap steel first and then adding iron must be adopted. After adding scrap steel, the converter should first be shaken down to more than 90°, so that the scrap steel does not pour out of the furnace mouth, and then shaken up to 45°. The purpose is to complete the replacement of cold-hot furnace gas in the furnace and reduce the temperature in the furnace. At this time, a large amount of high-temperature furnace gas is observed to be discharged from the furnace mouth, and the temperature of the furnace lining is significantly reduced. Repeat this operation once and observe the brightness of the furnace lining. If the brightness is high, it means that the temperature is high. The operation can be repeated until the furnace lining is dark red.

The four-step control method of slag splashing and furnace protection can reasonably control every link of the smelting process operation, improve the effect of slag splashing and furnace protection, and achieve the purpose of ensuring the stability of the converter furnace type.

Furnace type control is mainly based on the maintenance and control of the converter lining erosion, adhering to the furnace protection principle of “slag splashing as the main and material supplement as the auxiliary”. Continuously optimize the converter slag splashing and furnace protection process, improve the effect of slag splashing and furnace protection, summarize the four-step control method of converter steelmaking slag splashing and furnace protection “slag making-slag adjustment-slag splashing-slag solidification”, and actually promote it in steelmaking production. The converter furnace life is stable at more than 20,000 furnaces, and the furnace type control is reasonable, which meets the needs of various reactions in the steelmaking process to proceed smoothly, ensuring the stability of converter steelmaking production and creating considerable economic benefits.

The slag splashing furnace protection process uses the oxygen lance system of the converter to switch oxygen to nitrogen as the slag splashing gas source, and the supersonic nitrogen jet formed by the oxygen lance nozzle splashes the adjusted slag after steel tapping onto the inner wall surface of the converter, sintering to form a high-melting-point splashing slag layer to resist the erosion of high-temperature molten steel and slag, so as to achieve the purpose of increasing the service life of the converter.

Principle of slag splashing furnace protection process: During the steelmaking process, the oxides formed by the oxidation of molten iron, slag-making agents, and melted refractory materials combine to form slag. The slag splashing furnace protection uses high-pressure nitrogen to splash the slag left in the furnace after steel tapping onto the furnace lining to form a splashing slag layer, which plays a role in protecting the lining for the next furnace smelting. Therefore, the converter terminal slag must not only meet the requirements of the smelting process, but also meet the conditions for slag splashing furnace protection, that is, it is easy to splash onto the furnace lining. The slag splashed onto the furnace lining should be able to combine well with the furnace lining and have a certain ability to resist high-temperature erosion. Its process principle can be summarized as “splashing, sticking, and erosion resistance”.

Determination of basic parameters of the four-step control method for slag splashing and furnace protection: The four-step control method for slag splashing and furnace protection is the specific application of the slag splashing and furnace protection process in the actual steelmaking operation process. The purpose is to improve the slag splashing and furnace protection effect. The slag making step is the basis, which provides qualified slag for slag splashing and furnace protection; the slag adjusting step is the means, which adjusts the slag that is not suitable for slag splashing to the slag that meets the requirements; the slag splashing step is the key, which splashes the appropriate slag evenly onto the furnace lining to protect the furnace lining; the slag solidification step is to ensure that the splashed slag layer improves the strength and superheat as well as the erosion resistance of the splashing slag layer through cooling and sintering.

4. Improvement of slag splashing furnace protection technology and furnace type control

Converter steelmaking now adopts the operation of adding scrap steel first and then adding molten iron. Due to the large amount of scrap steel added, large pits will appear on the charging side (large surface) of the converter; due to low iron consumption, high TFe of the final slag, low alkalinity, serious scouring on both sides of the small surface of the steel tapping, especially the lower side of the steel tapping port will be eroded and deep pits will appear. Whether the iron block or the steel bar head can be pasted on the furnace lining after filling is the key link. The final slag composition and alkalinity determine whether the iron block and the steel bar head can be smoothly pasted on the furnace lining. Therefore, the appropriate slag composition and alkalinity must be adjusted.

4.1. Selection of final slag

The viscosity of the final slag decreases with the increase of Fe0 content in the slag and increases with the increase of alkalinity. For the technology of using iron blocks to fill large surfaces and steel bar cut heads to fill small surfaces, the final slag cannot be too thin, and the thin slag cannot stick: the thick slag cannot be completely immersed, and it also cannot stick, and it is easy to fall off, so it is necessary to choose a suitable slag.

The effect of iron block and steel bar head filling furnace is closely related to the basicity and TFe content of final slag. The effect is best when the basicity of final slag is appropriate and the final slag is not oxidizing. At this time, the final slag has good fluidity and can penetrate into the iron block and steel bar head to form a skeleton and form a good eutectic with the furnace lining. The final slag forms C2S and periclase minerals with high melting points during the cooling and solidification process, which has a particularly obvious protective effect on the furnace lining. When the slag viscosity is high, the fluidity is poor, the iron block is not firmly bonded to the furnace lining, and it is easy to fall off when the slag splashes, which is not effective.

4.2. Control of TFe in final slag

The main effect of Fe0 in final slag on the effect of furnace repair is that Fe0 can form low-melting-point eutectic compounds with Ca0, MgO, Si02, etc. in the slag, thereby reducing the effect of furnace repair. On the other hand, the high FeO content in the slag promotes the decarburization of the furnace lining bricks and the penetration of the slag into the furnace lining, thereby accelerating the erosion of the furnace lining. In practice, it is found that when the final carbon is controlled at 0.08%, the Fe0 content in the slag is about 15% to 17%. If post-blowing occurs, the iron oxide in the slag is as high as 20%. At this time, the slag is not suitable for furnace repair with iron blocks. Using lightly burned dolomite to replace part of the lime to make slag, increase the MgO content in the slag, and make the MgO content reach saturation, which can effectively reduce the erosion of the slag on the furnace lining.

4.3. Practice of using pig iron blocks and steel bar heads to repair the furnace

The conventional method of repairing the converter is to splash slag to protect the furnace. However, when large pits appear on the large surface of the furnace body and deep pits appear on the small surface, splashing slag to protect the furnace is no longer effective. At this time, the furnace must be stopped to repair the large and small surfaces. Conventional repair methods include tiling, filling materials, spraying, etc. No matter which method is used, the furnace must be stopped for operation and a certain sintering time is required, which often causes the casting machine to stop, seriously affecting the effective operation rate of the converter. The advantage of using pig iron blocks and steel bar heads to repair the furnace is that the time is very short, the production rhythm can be flexibly adjusted, thereby ensuring the continuity of production and greatly reducing the cost of repairing refractory materials.

The specific operation steps of pig iron block repairing large surfaces are as follows:

(1) Before deciding to repair the furnace, relevant personnel should be notified to take corresponding measures, such as notifying the continuous casting to reduce the pulling speed in advance, and the gun operator in front of the furnace should control the end point well, the end point C% ≥ 0.08%, R controlled at 2.7~2.8, the end point slag should not be too thin or too sticky, and the slag retention should be controlled at 3~5t.

(2) After steel is tapped, do not splash slag and shake the furnace directly. Shake the furnace body to the scrap steel adding position at 20-30 degrees, then command the overhead crane to add 1.5-2 tons of pig iron blocks, and continue to shake the furnace until the furnace mouth is level with the ground, ensuring that the iron blocks are just filled in the large surface pit and the slag does not flow out of the furnace mouth. Let it stand for 3-4 minutes, and then lift the furnace.

(3) After lifting the furnace, start splashing slag. After splashing for 2-3 minutes according to the normal slag splashing procedure, load scrap steel normally, add iron, and smelt normally.

The specific operation steps for filling the small surface of the steel bar head are as follows:

(1) Before deciding to fill the furnace, notify the relevant personnel to take corresponding measures, such as notifying the continuous casting to reduce the pulling speed in advance, and the assistant in front of the furnace should control the end point well, the end point C% ≥ 0.08%, R is controlled at 2.7-2.8, the end point slag is required to be neither too thin nor too sticky, and the amount of slag left is controlled at 3-5 tons.

(2) Notify the furnace filling personnel to bring 1.5-2 tons of steel bar heads to the 16m platform silo for standby.

(3) After steel is tapped, do not splash slag and shake the furnace directly. Shake the furnace body to the rear position of the furnace at 30-40 degrees. Then, the furnace shaker will add 1.5-2t of steel bar heads and continue to shake the furnace to the steel tapping position. Ensure that the slag does not flow out of the steel tapping port. Let it stand for 3-4 minutes and then lift the furnace.

(4) After lifting the furnace, start splashing slag. After splashing for 2-3 minutes according to the normal slag splashing procedure, load scrap steel and add iron normally, and smelt normally.

5. Effect of use

After using the technology of pig iron blocks, steel bar heads to supplement the furnace and splash slag to protect the furnace, the direct effect is that the production efficiency of the converter has been greatly improved, the operating rate has increased from the original 90% to 95%, and the time for supplementing the converter has been reduced from the original 45min to the current 6-8min. The monthly output has increased by 5,000-800 tons, the accident rate has also been greatly reduced, and the cost of refractory materials has been significantly reduced.

6. Conclusion

The technology of using pig iron blocks and steel bar cutting heads to fill the furnace and splash slag to protect the furnace adopted by the steel mill has been very mature through its application in practice. This technology has significant effects on increasing steel production, accelerating the smelting rhythm of the converter and reducing the cost of refractory materials. It can make full use of the gaps in production to fill the large and small surfaces of the converter. The method is flexible and can be regarded as a supplement to the splash slag protection technology. It is worth promoting and applying in other units.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking