Installation Considerations for Tundish Integral Stopper Rods

The tundish integral stopper rod is a core control component in the continuous casting process. Its installation quality directly impacts steel flow stability, mold level control accuracy, and production safety. Based on industry practice and technological innovation, this article systematically outlines the key technical points for integral stopper rod installation, providing a practical, operational guide for steelmakers.

01 Preparatory Preparations Before Installation

1. Pretreatment of the Stopper Rod Body

Drying: The stopper rod must be dried in a drying oven at 200-250°C for at least 24 hours, ensuring a moisture content of ≤0.5% to prevent cracking during the drying process. For example, Panzhihua Iron and Steel Corporation has reduced its stopper rod breakage rate by 37% by strictly controlling the drying curve.

Defect Screening: Ultrasonic testing is used to detect cracks, focusing on the transition zone between the rod head and the rod body and the metal connecting rod connection. A steel mill once failed to detect a 0.3mm microcrack, resulting in spalling of the stopper rod head during casting and causing steel leaks. Coating Protection: A 0.2-0.3mm thick anti-oxidation coating, primarily composed of borates, is sprayed onto the surface of the aluminum-carbon stopper rod. This coating extends high-temperature service life by 15%-20%.

2. Mechanism Status Verification

Opening and Closing Mechanism Calibration: Measure the stroke error of the lifting mechanism to ensure a 50-60mm opening and closing stroke with a repeatability accuracy of ≤0.5mm. One company installed a laser displacement sensor to control stroke deviation within ±0.3mm.

Lubrication System Maintenance: Use molybdenum disulfide-based grease to lubricate the guide rails at three points, ensuring a starting torque of ≤50 N·m.

Argon System Leak Testing: Use a helium mass spectrometer leak detector to inspect the stopper rod’s argon blowing channel. The leak rate must be ≤1×10⁻⁹ Pa·m³/s to prevent secondary oxidation caused by air ingestion during casting.

02 Key Control Points in the Installation Process

1. Precise Verticality Control

Three-Dimensional Positioning Method: Use a laser plummet to establish a datum for the nozzle centerline. Ensure the stopper rod installation verticality deviation is ≤0.5°. A special steel mill used this method to reduce mold level fluctuation from ±3mm to ±1mm.

Dynamic Grinding Process: When the stopper is open, deflect it 2-3mm toward the mechanism and rotate it forward and backward for 3-5 turns at a torque of 5-10 N·m. This creates a 0.1-0.2mm wear mark on the contact surface, reducing the friction coefficient by 30%.

2. Connection Strength Assurance

Threadlocking Technology: Anaerobic adhesive is applied to the threads of the metal connecting rod, achieving a shear strength of ≥25 MPa after curing. Using this measure, one company reduced thread loosening from 18% to 2%.

Dual Fixing Mechanism: A combination of metal pins and threads is used for fixing. The metal pins must have a shear strength of ≥200 kN, and the threaded connection preload is controlled within the range of 80-120 kN·m.

3. Environmentally Adaptable Design

Thermal Protection Structure: A 10mm thick ceramic fiberboard is installed on the mechanism housing to reduce the external surface temperature from 350°C to 120°C, extending the life of the hydraulic components by 2.3 times. Cooling System Optimization: Adding an 8mm diameter cooling air pipe to the front cover, with the argon flow controlled at 5-8 L/min, can reduce the internal temperature of the mechanism by 80-100°C.

03 Post-Installation Quality Verification System

1. Static Testing

Smoke Test: Place a smoke cake at the bottom of the nozzle and observe the smoke emission from the upper portion. The tightness must be at least 95% with no leakage. One steel plant improved the tightness from 92% to 98% by improving the curvature radius of the plug head.

Geometric Parameter Measurement: Use a three-dimensional coordinate measuring machine to check the coaxiality of the stopper rod and the nozzle. The deviation must be ≤1mm, and the end-face clearance must be ≤0.5mm.

2. Dynamic Testing

Simulated Casting Test: Perform no-load operation at a casting speed of 1.2m/min. Verify that the lifting mechanism response time is ≤0.8s, with no sticking or abnormal noise.

Hot Verification: When the tundish is baked to 1100°C, check the thermal expansion compensation of the stopper rod to ensure the reserved clearance is within the 3-5mm range.

04 Typical Fault Prevention and Treatment

1. Accelerated Erosion

Material Optimization: Using a MgO-Al₂O₃-C composite rod tip for calcium-treated steel grades can reduce the erosion rate by 40%. After implementation at one company, the service life of the stopper rod was extended from 6.5 hours to 9.2 hours.

Process Control: Strictly control the superheat of the molten steel between 25-40°C. If the superheat exceeds 50°C, an emergency replacement plan must be initiated.

2. Mechanical Failure Cases

Deformation Correction: For tundishes used more than 50 times, a laser tracker is used to measure the deformation of the tundish wall. If the deviation exceeds 3mm, mechanical correction or scrapping is required.

Hydraulic System Maintenance: Establish a regular hydraulic oil testing system. When the particle contamination level exceeds NAS Level 8, the filter element must be replaced and the pipeline flushed.

Intelligent Monitoring System: Integrates strain sensors and temperature probes to monitor the stress status of the stopper rod in real time. A pilot project has reduced unplanned downtime by 65%. 3D printing technology: Using selective laser melting to manufacture metal connecting rods increases material utilization from 35% to 82% and reduces delivery cycles by 70%.

Nanocoating application: Depositing an Al₂O₃-SiC nanocomposite coating on the stopper rod surface increases thermal shock resistance from 5 to 12 times.

The installation of the integral tundish stopper rod is a systematic project involving materials science, precision mechanics, and thermal engineering. By implementing standardized operating procedures, introducing intelligent testing methods, and continuously optimizing material processing, the safety and economic efficiency of continuous casting production can be significantly improved. It is recommended that companies establish an installation quality database and utilize the PDCA cycle for continuous improvement to build technological barriers in the face of fierce market competition.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook