The steel industry serves as a critical benchmark for a nation’s overall industrial capability, playing a pivotal role in safeguarding major infrastructure projects, elevating manufacturing standards, promoting energy efficiency, and driving technological advancement across related sectors. In recent years, domestic steel enterprises have intensified R&D investment and process upgrades. While rapid growth in steel output and product diversification has been achieved, certain high-end specialty steels—such as bearing steels for high-speed rail and landing gear steels for aerospace applications—remain heavily import-dependent.
To address this challenge, China’s Ministry of Industry and Information Technology (MIIT) incorporated high-grade bearing steel and 39 other premium steel grades into the Key New Materials First Batch Application Demonstration Guidance Catalog in 2019, offering targeted policy support for these materials. The key to breakthroughs in these steel grades lies in the precise control of non-metallic inclusions. When inclusions exist in unfavorable sizes, morphologies, and distributions, they disrupt the continuity and integrity of the steel matrix, severely impairing steel quality and performance.
Extensive research has been devoted to improving inclusion removal efficiency, yielding advanced techniques such as ultra-low oxygen smelting and inclusion plasticization. While these innovations effectively reduce inclusion count and mitigate their harm, complete control over all inclusion sizes and distributions remains elusive. This demonstrates that for high-end steels with long production routes and multiple process stages, precise inclusion control requires contributions from multiple coordinated factors.
Further tracking research into inclusion sources has confirmed that ladle lining refractory materials—which remain in continuous, large-area contact with molten steel throughout the entire refining process—are among the primary factors governing inclusion size and distribution. As secondary refining and alloying processes account for an increasing share of the steelmaking workflow, the importance of ladle working lining refractories has become ever more prominent, and their influence on non-metallic inclusions in steel cannot be overlooked.
Background: Evolution of Ladle Lining Refractory in China
Chinese ladle lining refractory materials have continuously evolved alongside developments in secondary refining technology. Over recent decades, metallurgical and materials researchers have iteratively updated design philosophies and developed multiple ladle lining refractory systems to meet the demands of different refining eras. These systems include:
- High-alumina refractories (based on natural bauxite synthesis)
- Carbon-composite refractories
- MgO-Al₂O₃ carbon-free refractories
- CaO-based refractories
High-alumina refractories have gradually been phased out from refining ladle linings due to their short service life and poor high-temperature performance—including poor thermal shock resistance, severe skull build-up, and weak slag corrosion resistance. The remaining systems are still in service but each carries inherent challenges: carbon pickup from carbon-composite refractories, thermal shock resistance issues in MgO-Al₂O₃ carbon-free refractories, and hydration problems in CaO-based refractories. These shortcomings can prevent refining processes from achieving expected results. Furthermore, the interface reactions between active refractories and molten steel during refining inevitably affect non-metallic inclusions in steel.
Effect of Current Mainstream Ladle Lining Refractory on Non-Metallic Inclusions
In actual refining operations, the ladle lining refractory contacts molten steel over a large surface area in real time. Under the combined action of high temperature and stirring, molten steel penetrates the refractory and triggers interface reactions, leading to progressive erosion of the refractory and alteration of molten steel composition. The degree of erosion and the impact on inclusions vary depending on refractory composition and refining process conditions.
Understanding how ladle lining refractory materials affect steel inclusions is not only critical for inclusion control in metallurgical industry but will also guide future refractory development. The following sections review and summarize two mainstream refractory types in current service: MgO-based refractories and Mg-Al refractories.
Effect of MgO-Based Ladle Lining Refractory on Non-Metallic Inclusions
Effect on Inclusions in Al-Killed Steel
Metallic aluminum is a widely favored deoxidizer owing to its low cost, strong oxygen affinity, and fast deoxidation kinetics. Aluminum deoxidation can reduce total oxygen content to extremely low levels, making it the deoxidizer of choice for steels with strict total oxygen requirements—typical examples include bearing steel, IF steel, and pipeline steel. Extensive research has been conducted on the effect of MgO-based ladle lining refractory on inclusions in Al-killed steel.
Studies of the reaction mechanism between MgO-C refractory and Al-killed steel revealed that, even without any magnesium addition, both MgO and MgO·Al₂O₃ inclusions appeared in the steel, and a thin magnesia-alumina spinel layer formed at the MgO-C refractory/molten steel interface. The MgO-C ladle lining refractory dissolves magnesium into steel by carbon reduction of its own MgO, which then reacts with dissolved aluminum to form magnesia-alumina spinel inclusions, as shown in Equations (1) and (2):
(1) MgO + C = Mg(g) + CO(g)
(2) [Mg] + 2[Al] + 4[O] = MgO·Al₂O₃
When aluminum deoxidation is applied, the molten steel contains substantial dissolved aluminum, which also participates in dissolving MgO from the ladle lining refractory via a displacement reaction. Studies of MgO-C refractory interaction with Al-killed steel found that MgO in the refractory reacts with dissolved aluminum in the melt through a displacement reaction, simultaneously generating dissolved magnesium and MgO·Al₂O₃ inclusions (Equation 3):
(3) 4MgO + 2[Al] = 3[Mg] + MgO·Al₂O₃
The two dissolution pathways differ in elemental distribution at the interface. Where dissolved aluminum drives the displacement reaction, a magnesia-alumina spinel layer forms at the reaction interface (Fig. 1(a)). Where carbon reduction is the dominant mechanism, no spinel layer is observed at the refractory/steel interface (Fig. 1(b)).

The evolution of inclusion chemistry with reaction time is shown in Fig. 2. Prior to the experiment, inclusions in the melt consisted primarily of Al₂O₃ from aluminum deoxidation. As reaction time increased, the MgO mass fraction within inclusions rose progressively. After more than 3.5 minutes of reaction, the dominant inclusion type became MgO·Al₂O₃.

To isolate the effect of MgO dissolution independent of carbon, the dissolution behavior of pure MgO refractory in Al-killed steel was also investigated. MgO rods were immersed in Al-killed molten steel at varying reaction times. Results showed:
- A thin MgO·Al₂O₃ layer formed at the MgO refractory/molten steel interface (Fig. 3(a))
- In the early stages, MgO·Al₂O₃ phase appeared at the edges of Al₂O₃ inclusions (Fig. 3(b))
- With prolonged reaction time, all Al₂O₃ inclusions transformed into angular MgO·Al₂O₃ inclusions (Fig. 3(c))

This confirms that at refining temperatures, dissolved aluminum reacts with the MgO ladle lining refractory to form an MgO·Al₂O₃ layer and dissolved magnesium (Eq. 3), which further reacts with existing Al₂O₃ inclusions to yield MgO·Al₂O₃ inclusions (Equation 4):
(4) [Mg] + [O] + Al₂O₃ = MgO·Al₂O₃
Oxygen activity was identified as the key variable controlling whether MgO refractory generates dissolved magnesium and promotes Al₂O₃-to-spinel transformation. At very low oxygen activity (≤0.0001%), the refractory generates substantial dissolved magnesium, driving the Al₂O₃-to-MgO·Al₂O₃ transformation (Fig. 4). At sufficiently high oxygen activity (≥0.0500%), Al₂O₃ inclusions show no compositional change.

In industrial refining practice, both MgO-bearing refining slag and MgO-based ladle lining refractory supply dissolved magnesium to molten steel. A kinetic model comparing their relative contributions yielded magnesium transfer rates of 2.18 × 10⁻⁴ m/s for MgO refractory, 5.0 × 10⁻⁴ m/s for MgO-C refractory, and 6.3 × 10⁻⁴ m/s for MgO-bearing refining slag. Although MgO-bearing slag delivers magnesium faster per unit area, the contact area of the ladle lining refractory with molten steel is approximately four times that of the slag/steel interface. Therefore, within the same time frame, MgO-based ladle lining refractory exerts a greater driving force for converting Al₂O₃ inclusions to MgO·Al₂O₃ than MgO-bearing slag.
In summary, MgO-based ladle lining refractory dissolves magnesium into steel more effectively than refining slag and drives the transformation of Al₂O₃ inclusions to MgO·Al₂O₃ inclusions.
Effect on Inclusions in Si-Mn Deoxidized Steel
For special-purpose medium-to-high carbon long products—such as tire cord steel, wire saw steel, and spring steel—Si-Mn composite deoxidation is typically employed to avoid wire breakage caused by Al₂O₃ inclusions during downstream cold-drawing. This approach controls inclusion morphology to achieve superior plasticity.
Research into the independent effect of MgO refractory on inclusions in Si-Mn deoxidized steel found that with increasing reaction time, the melting points of the original SiO₂-Al₂O₃-MnO and SiO₂-Al₂O₃-CaO system inclusions both decreased, ultimately stabilizing below 1,500°C (Fig. 5).

Therefore, while MgO-based ladle lining refractory promotes the formation of MgO·Al₂O₃ inclusions in Al-killed steels—which is detrimental to steel properties—its use in Si-Mn deoxidized steel actually favors the formation of low-melting-point inclusions, thereby reducing inclusion-induced harm to steel performance.
Effect of Mg-Al Refractory on Non-Metallic Inclusions
Effect on Inclusions in Al-Killed Steel
Mg-Al refractories offer long service life and excellent stability, combining superior overall performance with the elimination of carbon pickup associated with MgO-C bricks. They are therefore widely applied in Al-killed steel production. Research by Deng Z. et al. on the effect of Mg-Al ladle lining refractory on inclusions in Al-killed low-alloy steel showed minimal influence, with no promotion of Al₂O₃-to-spinel transformation. This is because the MgO activity in Mg-Al refractory is very low (~0.06), making it difficult to react with molten steel and generate dissolved magnesium in amounts sufficient to affect inclusions.
However, in Al-killed medium-manganese steel, Mg-Al ladle lining refractory undergoes a displacement reaction with dissolved manganese (Equation 5), forming a (Mn,Mg)O·Al₂O₃ transition layer at the refractory/steel interface. As reaction time increases, the erosion layer thickens and manganese diffuses progressively from the refractory edge toward the center (Fig. 6). When this altered interface layer is abraded by the flowing melt, it detaches from the refractory matrix and enters the steel as (Mn,Mg)O·Al₂O₃ inclusions (Fig. 7).
(5) MgO·Al₂O₃ (refractory) + [Mn] = MnO·Al₂O₃ (refractory) + [Mg]


In summary, while Mg-Al ladle lining refractory exerts minimal effect on inclusions in Al-killed low-alloy steel, it undergoes significant interfacial reactions with Al-killed medium-manganese steel, substantially affecting inclusion morphology and chemistry.
Effect on Inclusions in Si-Mn Deoxidized Steel
Mg-Al refractories are also applied in Si-Mn deoxidized steel production due to their excellent high-temperature service performance. Dynamic interaction experiments between Mg-Al ladle lining refractory and Si-Mn alloy steel demonstrated that at high temperature, the refractory is eroded by Si-Mn alloy steel and a liquid-phase transition layer forms. Under dynamic steel flow, this transition layer emulsifies with the melt, causing steel droplets to disperse within the liquid transition zone—allowing molten steel to penetrate the interface layer and continue reacting with the refractory. This cyclic mechanism leads to progressive erosion of the refractory (Fig. 8), and the liquid transition layer can enter the steel as inclusions when subjected to melt agitation.

When studying the interaction between Mg-Al ladle lining refractory and 95Cr wire saw steel, researchers found that the Mg-Al refractory had a certain inclusion-removal capability and was able to shift the melting point distribution of most inclusions in the wire saw steel into the low-melting-point zone below 1,300°C (Fig. 9).

In Al-killed low-alloy steel, the low MgO activity of Mg-Al ladle lining refractory precludes significant magnesium dissolution and inclusion impact. In Al-killed medium-manganese steel, the manganese content drives significant interfacial reactions, generating a liquid transition layer that delivers inclusions to the steel. In Si-Mn deoxidized steel, a similar transition layer forms and introduces inclusions into the steel, albeit while lowering inclusion melting points to some degree.
Effect of Novel Ladle Lining Refractory on Non-Metallic Inclusions
Although the current mainstream ladle lining refractory materials satisfy service life requirements under present-day refining technology, they continue to present challenges in structural integrity, high-temperature service performance, and harmless treatment of inclusions in steel. Future ladle lining refractory should therefore not only provide stable high-temperature service performance but should also actively purify the molten steel.
As research into refractory/molten steel interface reactions has deepened, it has been found that CaO-based refractories can modify—and even adsorb and remove—Al₂O₃, SiO₂ inclusions and phosphorus and sulfur from steel. For example, free CaO reacts with Al₂O₃ at refining temperatures to form low-melting-point compounds Ca₁₂Al₁₄O₃₃ (C12A7) and Ca₃Al₂O₆ (C3A)—both liquid at refining temperatures of 1,600–1,700°C—according to Equations (6) and (7):
(6) 12CaO + 7Al₂O₃ = Ca₁₂Al₁₄O₃₃ (7) 3CaO + Al₂O₃ = Ca₃Al₂O₆
Liquid inclusions at refining temperature not only coalesce and grow more readily—increasing the probability of flotation removal—but also reduce the risk of nozzle clogging. However, the hydration susceptibility of CaO has long limited the industrial adoption of CaO-based ladle lining refractory.
The research group of the present authors departed from the conventional approach of mechanically blending natural raw materials and conducted systematic research on CaO-MgO-Al₂O₃ (CMA) materials from the perspective of compositional regulation and structural matching. CA6 as a ladle lining refractory offers multiple advantages: high melting point (1,875°C), good stability in high-temperature reducing atmospheres, strong resistance to highly basic slag attack, and low wettability with molten metal—eliminating chemical reactions with the melt. By mastering the synthesis principles of CA6, dense CA6 refractory (density: 3.10 g/cm³) was successfully fabricated for the first time. Building on this foundation, through the combination of M-blocks (magnetoplumbite blocks) and S-blocks (spinel blocks), two CaO-MgO-Al₂O₃ (CMA) ternary functional raw materials were synthesized: CaMg₂Al₁₆O₂₇ (CM2A8) and Ca₂Mg₂Al₂₈O₄₆ (C2M2A14), with densities of 3.66 and 3.71 g/cm³ respectively. These materials exhibit structural stability and resolve the hydration problem of traditional CaO-containing refractories.
Comparative slag erosion tests (basicity 3.2) were conducted between CMA material (C2M2A14) and corundum-spinel castable. After 3 hours of erosion by high-basicity slag at 1,550°C, a significant difference in erosion depth was observed: the C2M2A14 erosion layer was only 179 μm thick, versus 406 μm for the corundum-spinel castable. The C2M2A14 erosion layer was composed of dense CA and CA2 phases with no slag penetration, effectively inhibiting slag attack. In contrast, the corundum-spinel castable erosion layer contained substantial slag constituents alongside CA and CA2 phases, with slag continuing to attack the refractory matrix over time (Fig. 10).

Furthermore, the effect of CMA-series materials versus corundum-spinel castable on inclusions in Al-killed steel in the presence of refining slag was compared. Within 40 minutes of reaction—consistent with typical industrial refining time—the inclusions in steel refined with the CMA ladle lining refractory were primarily MgO·Al₂O₃ particles smaller than 5 μm. In contrast, the corundum-spinel castable yielded larger MgO·Al₂O₃ inclusions wrapped in MnS. This demonstrates that within the typical industrial refining window, CMA material resists slag erosion, shows low wettability with molten metal, introduces no CaO-type inclusions into the steel, and adsorbs sulfur—preventing sulfide precipitation during solidification.
When the experiment was extended to 50 minutes to investigate the effect of the CMA erosion/transition layer on inclusions, the CMA erosion layer thickness stabilized at approximately 150 μm, and low-melting-point CaO-MgO-Al₂O₃ composite inclusions appeared in the steel, primarily within the 1–4 μm size range. This indicates that with further slag penetration, the CMA ladle lining refractory forms a high-temperature-stable protective transition layer that inhibits further slag ingress. Simultaneously, CMA material leverages the slag erosion reaction to release Ca₁₂Al₁₄O₃₃ (C12A7), modifying MgO·Al₂O₃ inclusions into small, low-melting-point CaO-MgO-Al₂O₃ composite inclusions—functioning in a manner analogous to refining slag.
The successful development of CMA material provides a new paradigm for future refractory advancement. The research group has partnered with refractory manufacturers to initiate industrial-scale production and has achieved pilot-scale industrial trials at several steel plants. In the near future, novel functional ladle lining refractory materials exemplified by CMA are expected to provide stronger support for advanced refining technology and jointly advance the domestic production of high-quality steels.
Conclusions
- MgO-based ladle lining refractory dissolves magnesium into Al-killed steel, driving the transformation of Al₂O₃ inclusions to MgO·Al₂O₃ inclusions. However, in Si-Mn deoxidized steel, this type of refractory actually favors the formation of low-melting-point inclusions.
- Mg-Al ladle lining refractory has minimal effect on inclusions in Al-killed low-alloy steel but undergoes significant interfacial reactions with Al-killed medium-manganese steel, forming an altered layer that delivers inclusions to the steel. In Si-Mn deoxidized steel, it behaves similarly—transporting inclusions through the transition layer—while lowering inclusion melting points to some degree.
- Future ladle lining refractory materials should break free from conventional development thinking, moving beyond mere service life extension to incorporate functional performance: removing or rendering harmless inclusions and impurity elements in steel under stable service conditions without contaminating the melt. The successful development of CMA material offers a new direction for future ladle lining refractory advancement.
FAQ
What is ladle lining refractory and why does it affect non-metallic inclusions in steel?
Ladle lining refractory refers to the working lining materials installed inside a steel ladle that remain in continuous, large-area contact with molten steel during secondary refining. At high temperatures and under stirring, molten steel penetrates the refractory and triggers chemical interface reactions. These reactions erode the refractory, alter the composition of molten steel, and directly influence the type, morphology, size, and distribution of non-metallic inclusions—making the choice of ladle lining refractory one of the most critical factors in inclusion control.
How does ladle lining refractory erosion contribute to large exogenous inclusions in steel?
Ladle lining refractory erosion contributes to exogenous inclusions through two mechanisms: (1) mechanical spalling—under the physical impact and flow of molten steel, fragments of the altered interface layer or refractory matrix detach and enter the melt as large macro-inclusions; and (2) chemical introduction—dissolved species (Mg, Ca, Al, Mn) released from the refractory through interface reactions precipitate as new inclusion phases within the steel. Both mechanisms can generate inclusions in harmful size ranges that are difficult to remove by flotation.