Erosion Mechanism of LF Ladle Refractory Materials in the Molten Pool Zone: A Case Study from a Steel Plant

Secondary refining (Ladle Metallurgy) is the primary process in modern steelmaking plants for deep deoxidation, desulfurization, inclusion removal, and alloying of molten steel. In today’s steel industry, the performance of LF ladle refractory materials directly affects ladle campaign life, steel cleanliness, operating cost, and production stability. Considering the different corrosive media acting on various parts of the LF refining ladle, the working lining is generally divided into the slag line zone and the molten pool zone.

The slag line area, subjected to severe erosion by oxide slag, typically employs MgO-C (Magnesia-Carbon) bricks with a carbon content of 12–18 wt%. Due to the rapid melting loss of slag line refractories caused by high-basicity refining slag, the slag line usually requires at least one replacement during a single ladle campaign. Therefore, selecting high-performance steel ladle refractory bricks with strong slag corrosion resistance is critical for extending service life.

Refractories in the molten pool zone are mainly eroded by molten steel during the refining process. Before hot repairs are conducted after casting, the slag must be dumped. The refractories on the slag-dumping surface are primarily affected by chemical corrosion and physical scouring from the slag. Materials commonly used for the molten pool zone include Magnesia-Alumina Carbon (MgO-Al2O3-C), Alumina-Magnesia Carbon (Al2O3-MgO-C), and Carbon-Free Alumina-Magnesia refractories. These materials are widely applied as LF ladle refractory lining materials in modern refining operations.

During service, since the molten pool refractories are located in the lower-middle section of the ladle, replacement is difficult and the economic cost-effectiveness is generally low. Consequently, the service life of the molten pool zone largely determines the overall campaign life of the steel ladle. For this reason, improving the durability of ladle furnace refractory bricks has become an important topic for steel plants seeking longer campaign life and lower refractory consumption.

The wear mechanism of refractories is a complex issue; slag properties, operating temperatures, refractory composition, molten steel flow, and metallurgical conditions all influence the erosion process. On-site, the damage to the ladle lining is the result of the combined coupling of the temperature field, steel/slag flow fields, and chemical corrosion. Therefore, investigating the localized damage mechanisms of LF ladle refractory materials in the molten pool zone is not only a scientific exploration of refractory erosion theory but also provides significant practical guidance for steelmaking operations.

Site Investigation of LF Ladle Refractory Erosion

During the decommissioning and breakout process of a 180t BOF (Basic Oxygen Furnace) converter ladle at a steel plant, it was observed that the residual thickness of the molten pool bricks at the 12 o’clock position was significantly lower than that of the surrounding bricks (see Figure 1). This localized erosion restricted the further extension of the ladle campaign life (see Table 1).

The basic operating conditions of the plant are as follows:

  • The metallurgical environment is 100% LF (Ladle Furnace) refining
  • the steel grades produced are primarily aluminum-killed steels
  • the refining slag has a relatively high basicity (see Table 2)
  • The internal structure of the ladle features purging plugs (permeable bricks) located at the 5 o’clock and 7 o’clock positions
  • During refining, the electrodes are inserted into the ladle at the 1 o’clock, 2 o’clock, and 6 o’clock positions (see Figure 2)
Residual thickness of molten pool bricks during ladle breakout
Figure 1: Residual thickness of molten pool bricks during ladle breakout

Table 1: Residual thickness of the ladle working lining (mm)

Layer12
o’clock
1
o’clock
3
o’clock
5
o’clock
6
o’clock
7
o’clock
9
o’clock
11
o’clock
Layer 1508010013011011012070
Layer 4609013015012012014090
Layer 770110150160125130160110

Table 2: Chemical composition of the on-site refining slag

Steel GradeCaOMgOSiO₂Al₂O₃Fe₂O₃Mn₂O₃
SPHC58.55.446.5924.960.42—

In modern secondary metallurgy, the interaction between molten steel flow and refractory lining plays a decisive role in the performance of steelmaking refractory materials.

It is well-known that there are typically three common locations for “weak points” (severe erosion) in a ladle:

Near the electrodes: The high temperatures generated by the electrodes accelerate the reaction between the slag/molten steel and the refractory materials.

Near the purging plugs: The bubbling/stirring action after the purging gas is activated intensifies the physical scouring of the refractories by the molten steel.

The slag-dumping surface: At the end of a ladle cycle, the residual steel and slag must be poured out. During this tilting process, the slag-dumping surface is subjected to intense scouring and chemical attack.

However, in this case, the weak point was not located at any of these conventional positions, making the investigation highly significant for understanding the failure mechanism of LF refining ladle refractories.

Used bricks were collected from both the weak direction and the non-weak direction of the molten pool (as shown in Figures 3 and 4), with effective residual thicknesses of 60 mm and 160 mm, respectively.

Observation revealed that a slag layer existed on the surface of the molten pool brick from the non-weak direction, while the brick from the weak direction had almost no slag layer. Parallel to the hot face, two cracks filled with slag were visible on the non-weak-direction brick surface. These findings provided important clues for analyzing the wear behavior of ladle refractory lining materials.

Schematic of the relative positions of graphite electrodes within the ladle
Figure 2: Schematic of the relative positions of graphite electrodes within the ladle
Morphology of the used brick from the 5 o’clock position of the ladle wall
Figure 3: Morphology of the used brick from the 5 o’clock position of the ladle wall
Morphology of the used brick from the 12 o’clock position of the ladle wall
Figure 4: Morphology of the used brick from the 12 o’clock position of the ladle wall

Testing and Analysis of Used Ladle Refractory Bricks

2.1 Testing Methods and Procedures

Samples measuring 25 mm × 25 mm × 25 mm were cut at 25 mm intervals from the hot face to evaluate physical and chemical properties. Microstructural analysis was performed on sections near the hot end to study the erosion characteristics of the ladle furnace refractory lining.

2.2 Physicochemical Analysis of Used Bricks

Table 3 presents the physical indicators of the samples at different distances from the hot face. It can be observed that in the 0–25 mm zone, there is little difference in the apparent porosity and bulk density between the molten pool bricks from the two directions. However, the bulk density of the sample from the weak direction is slightly higher.

In the 30–55 mm range, the bulk density of the weak-direction sample (2.80 g/cm³) is significantly higher than that of the non-weak direction (2.74 g/cm³), and its apparent porosity (14.8%) is markedly lower than that of the non-weak direction (16.2%).

This indicates that at the same distance from the hot face, the weak-point sample possessed higher density and lower porosity, suggesting that the molten pool bricks in the weak direction had a thinner slag penetration layer or decarbonized layer. Such characteristics are closely related to the service behavior of MgO-C refractory bricks used in LF ladles.

Apparent Porosity and Bulk Density of Samples at Different Distances from the Hot Face
Table 3: Apparent Porosity and Bulk Density of Samples at Different Distances from the Hot Face
Distance from Hot Surface / mmDirectionCaOMgOSiO₂Al₂O₃Fe₂O₃C
≤ 255 o’clock8.9358.165.7115.050.857.23
12 o’clock3.3566.604.1614.160.766.08
30 ~ 555 o’clock1.5766.585.0312.270.6910.9
12 o’clock1.2964.804.0714.120.6211.13
60 ~ 855 o’clock1.3065.974.7512.720.6811.0
12 o’clock

Table 4: Chemical Composition of Samples at Different Distances from the Hot Face

Table 4 shows the chemical indicators of the samples. It is evident that the CaO content gradually decreases as the distance from the hot face increases. Comparing samples at the same distance, the CaO content in the non-weak-point direction is higher than that in the weak-point direction. The CaO content of the original brick layer should be approximately 1.3 wt%. For the non-weak-point brick at the 5 o’clock position, the CaO content is 1.57% at a distance of 30–55 mm from the hot face, which is greater than 1.3%. This indicates that the slag penetration depth of the molten pool brick in the non-weak direction is at least 25 mm.

This demonstrates that slag penetration behavior is one of the key factors affecting the performance of secondary refining refractory materials.

2.3 Microstructural Analysis

Figure 5 shows the microstructure of the used molten pool brick from the 5 o’clock position. The hot face section is clearly divided into four layers: slag layer, reaction layer, decarbonized layer, and penetration layer.

The slag layer thickness was 3.4 mm, the reaction layer was 2.7–4.6 mm, and the decarbonized layer was 3.4 mm. High CaO content was also detected deeper from the hot face, indicating significant slag penetration.

The reaction layer on the surface of the 5 o’clock brick was relatively thick. The aggregates and matrix were sintered together, forming a dense structure with high strength. This dense layer acted as a barrier against further oxidation by oxygen and slag oxides while also improving erosion resistance of the ladle refractory bricks.

EDS analysis confirmed the formation of magnesia-alumina spinel:

​MgO+Al2O3→MgAl2O4

The formation of MgAl2O4 spinel indicates that under high-basicity slag conditions, alumina and magnesia react at high temperature to produce a stable high-temperature phase that effectively protects the refractory lining from further corrosion. This mechanism is particularly important for high-performance LF ladle refractory materials.

Microstructure of the used brick from the 5 o’clock position
Figure 5: Microstructure of the used brick from the 5 o’clock position(A. Slag layer; B. Reaction layer; C. Decarbonized layer; D. Penetration layer)
RegionMgOAl₂O₃SiO₂CaOFe₂O₃
Region 114.4327.889.1448.551.25
Region 283.5811.231.763.43—
Region 369.6215.049.034.361.39

Table 5: EDS Analysis of Different Regions in Figure 5

In contrast, the microstructure of the used molten pool brick from the 12 o’clock position revealed extremely thin slag, reaction, and decarbonized layers. The penetration layer was only about 2.5 mm thick. Unlike the 5 o’clock brick, the weak-direction brick failed to form a stable and dense reaction layer.

The reaction layer between the slag and the brick was discontinuous and porous. Chemical analysis showed that the CaO content dropped rapidly with increasing distance from the hot face, indicating shallow slag penetration.

In summary:

  • The 5 o’clock brick formed a dense and continuous reaction layer that effectively blocked slag penetration and molten steel erosion.
  • The 12 o’clock brick failed to form a stable protective layer and was repeatedly exposed to oxidation and molten steel scouring.

This resulted in a cyclic wear mechanism of:

Erosion→Oxidation→Erosion/Scouring

This cyclic damage mechanism is highly consistent with the typical erosion behavior of carbon-containing steel ladle refractory linings reported in refractory literature.

Microstructure of the used molten pool brick from the 12 o’clock position
Figure 6: Microstructure of the used molten pool brick from the 12 o’clock position (A. Slag layer; B. Reaction layer; C. Decarbonized layer; D. Penetration layer; E. Original brick layer)

Table 6: Chemical Composition of Rectangular Areas in Figure 6

RegionMgOAl₂O₃SiO₂CaOFe₂O₃
Region 17.6338.454.8245.963.13
Region 271.8012.069.455.481.22
Region 365.3916.8413.332.931.51
Region 476.6512.756.222.541.84
Region 572.0813.5211.811.341.26

Analysis of the Localized Erosion Mechanism

The formation of the dense reaction layer appears closely related to ladle operating practices.

After casting is completed and the ladle leaves the continuous casting platform, residual slag and molten steel must be dumped. During this process, the slag-dumping surface remains covered by slag. Although chemical corrosion intensifies, the slag layer also provides thermal shock buffering.

At the same time, the high-basicity slag reacts with the refractory bricks to form a dense and continuous protective reaction layer, preventing further attack by oxygen and slag.

However, at the 12 o’clock position, only a thin film of slag adheres to the refractory surface as the liquid level drops during casting. After casting, this area is exposed directly to air oxidation and thermal shock, making it difficult to form a dense protective layer.

During the subsequent refining cycle, the absence of protection allows the newly formed reaction layer to be quickly scoured away by molten steel, leading to accelerated erosion of the LF ladle refractory lining.

Conclusion and Optimization Recommendations for LF Ladle Refractory Materials

In response to the localized rapid erosion of molten pool bricks in a steel plant’s refining ladle, the erosion morphology and microstructure of used refractory bricks from different positions were systematically analyzed. The following conclusions were obtained:

The metallurgical operation process is the primary cause of localized rapid melting loss in LF refining ladles. The slag-dumping surface, being covered by steel slag, forms a dense reaction layer that inhibits further infiltration by air and slag while enhancing scouring resistance.

In contrast, the abnormal localized erosion on the non-slag-dumping surface is mainly caused by the loose and porous structure of the reaction layer between the refractory brick and slag, making it easier for molten steel to scour away the protective layer during subsequent refining cycles.

Coupled with cyclic metallurgical operations, the repeated process of:

  • Erosion
  • Oxidation
  • Erosion/scouring

becomes the fundamental wear mechanism of carbon-containing LF ladle refractory materials.

Based on the analysis above, the following optimization recommendations are proposed for improving the performance of steelmaking refractory materials:

1. Improve Refractory Bulk Density

Increase the bulk density of refractories on the non-slag-dumping surface to improve the compactness and stability of the reaction layer.

2. Enhance Hot Modulus of Rupture (HMOR)

Improve the HMOR of the refractory materials to strengthen resistance against molten steel scouring.

3. Improve Oxidation Resistance

Enhance the oxidation resistance of the refractory lining materials to reduce oxidation damage during LF refining operations.

4. Optimize Slag-Refractory Compatibility

Control refining slag basicity and slag composition to improve compatibility between slag and the ladle refractory lining.

5. Select High-Performance LF Refractory Bricks

Using high-density MgO-C bricks, alumina-magnesia carbon bricks, and advanced low-carbon refractory materials can significantly extend ladle campaign life and reduce refractory consumption costs in secondary steelmaking operations.

Why do molten pool refractories erode quickly in LF ladles?

Molten pool refractory erosion is mainly caused by molten steel scouring, slag penetration, oxidation, and thermal cycling. Poor reaction layer formation can accelerate refractory wear.

Why are MgO-C refractory bricks widely used in ladles?

MgO-C refractory bricks offer excellent slag resistance, thermal shock resistance, and high-temperature strength, making them ideal for slag line and molten steel contact areas.

How can the service life of ladle refractory lining be improved?

The service life can be improved by increasing refractory density, enhancing oxidation resistance, optimizing slag composition, and selecting high-performance LF refining ladle refractories.

Which factors affect steel ladle refractory brick performance?

Key factors include slag basicity, refining temperature, molten steel flow, refractory composition, thermal shock, and operational practices during secondary refining.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information