lmm@magnesiacarbonbricklmm.com

Introduction

With the rising demand for New Energy Vehicles (NEVs) and automotive lightweighting, the performance requirements for high-end 38MnV6 steel (non-quenched and tempered) have become increasingly stringent. These materials must achieve high fatigue strength while maintaining excellent machinability. Traditionally, sulfur control in steelmaking relies on high-basicity slag followed by vacuum iron sulfide (FeS) addition. However, this conventional method suffers from unstable sulfur yield, frequent composition deviations, and low production efficiency, making it difficult to meet the high purity and cleanliness requirements of modern high-grade steel.

To address these challenges, this study proposes an advanced micro-desulfurization technology during the LF refining process. Using the Mannesmann Index (MI) of refining slag composition as a theoretical basis, this method shifts metallurgical cleanliness control to earlier stages. Tailored for the EAF+LF+VD+CC (Electric Arc Furnace + Ladle Furnace + Vacuum Degassing + Continuous Casting) process, this refining strategy ensures thorough deoxidation while enabling precise sulfur control, significantly reducing alloy costs and improving the overall quality of sulfur-containing non-quenched and tempered steel.

Experimental Materials and Methods

Experimental Materials

The chemical composition specifications and the actual average composition of 38MnV6 sulfur-containing non-quenched and tempered steel are shown in Table 1. The metallurgical process employed is EAF + LF + VD + CC.

Actual Controlled Chemical Composition of 38MnV6 Molten Steel

Production Process Control

The EAF endpoint carbon mass fraction was controlled at above 0.10%, with the endpoint phosphorus mass fraction not exceeding 0.015%. Eccentric Bottom Tapping (EBT) was utilized to ensure slag-free tapping. Pre-deoxidation was performed by adding modified refining slag, Si-Mn alloy, and aluminum-cored wire to facilitate the early formation of large oxide inclusions, which float up more easily during the subsequent refining process. Slag carry-over during tapping was strictly prohibited. During the tapping process, 3–3.5 kg/t of lime and 3–3.5 kg/t of modified refining slag were added.

At the LF station, deoxidation was conducted by adding Si-Mn and aluminum shots. Diffusion deoxidation was performed by adding SiC powder to the slag surface to create a white slag. Continuous argon blowing and sufficient stirring were maintained throughout to promote the slag-steel reaction and the collision and flotation of deoxidation products. The refining slag composition was dynamically adjusted to ensure sufficient white slag refining time. Appropriately increasing the Al2O3 mass fraction in the slag system can enhance its capability to adsorb inclusions, thereby achieving thorough deoxidation. For sulfur-containing non-quenched and tempered steel, the molten steel must maintain a high sulfur content while having low oxygen levels; therefore, the refining slag must provide an excellent deoxidation effect while maintaining a low sulfur partition coefficient. For the VD stage, the vacuum degree was maintained at no more than 10 Pa for a holding time of over 12 minutes.

The experiment focuses on the timing of deoxidizer addition and its impact on slag composition during the refining process, further investigating the influence of refining processes on oxygen and sulfur control, as well as inclusion characteristics in sulfur-containing non-quenched and tempered steel.

Metallurgical Results

Oxygen Content Control

By shifting the deoxidation stage forward, the dissolved oxygen in the molten steel was successfully reduced from 100 ppm at EAF tapping to 35 ppm upon LF arrival, and further decreased to 10 ppm after the white slag refining stage.

Slag Composition Control and Effects

There is a functional conflict between the foaming performance and the refining performance of molten slag, particularly regarding the SiO2 content. As a surface-active agent, a SiO2 content above 20% yields optimal foaming effects, but at the expense of refining efficiency. In this study, the optimized composition for LF foaming refining slag was determined as: CaO 45%–60%, Al2O3 30%–40%,SiO2 10%–15%, MgO 5%–10%, and CaF2< 5%, with a Mannesmann Index (MI = CaO / (Al2O3 · SiO2)) of approximately 0.15.

Based on these results, refining slag compositions should be adjusted according to specific product requirements in industrial production. Processes prioritizing high desulfurization should be distinguished from those primarily focused on molten steel temperature adjustment to avoid a “one-size-fits-all” slag strategy. For grades with heavy desulfurization tasks like pipeline steel (low-sulfur steel), the MI should be above 0.25; whereas for carbon structural steels, the MI should be around 0.15 to leverage the advantages of slag foaming and improve thermal efficiency.

This study utilizes the Mannesmann Index as the theoretical basis (where an MI of ~0.15 significantly suppresses the desulfurization capability of the slag) to develop a “micro-desulfurization” slag system and process. This process stabilizes sulfur yield, eliminates the need for post-vacuum sulfur additions, reduces sulfur-related composition deviations, and enhances the effectiveness of post-vacuum soft stirring while reducing alloy costs by minimizing iron sulfide usage. Preliminary calculations for LF incoming slag (Fig. 1) show that high-MI slag (MI=1.6) requires 500kg of lime and 350kg of refining slag to reach an MI of 0.11 and enter the 1500°C melting zone. In contrast, low-MI slag (MI=0.28) only requires 200kg of lime and 400kg of refining slag, facilitating smoother control of the LF process.

Control process for rational slag modification with different initial slag compositions

In actual trials, the endpoint MI was controlled at 0.15. The slag compositions are listed in Table 2.

Slag Composition During Refining Process

Sulfur content variations are shown in Fig. 2: [S] was 0.020% at LF arrival, dropped to 0.014% after deoxidation, and reached 0.009% mid-refining. Feeding 3×90 kg of iron sulfide raised [S] to 0.035% at LF departure. After entering VD, [S] was 0.033% at the first sampling; after adding 35m of sulfur wire, [S] remained above 0.045% until the end of the vacuum process.

Changes in Steel Liquid [S] Content During Refining Process

Inclusion Analysis

Metallographic analysis was used to observe the inclusion distribution on the inner arc of the continuous casting billet under different MI values (Figs. 3 & 4).

Inclusion distribution on the inner arc of continuous casting billet with height low MI value

Comparison shows that after rapid deoxidation, finely dispersed Al2O3 serves as nucleation sites for MnS. Since no massive secondary sulfur addition was required, the size of MnS inclusions did not significantly increase. The improved distribution of fine, dispersed inclusions enhances machinability and promotes intragranular ferrite nucleation, improving overall quality.

Conclusions

(1) In the production of 38MnV6 sulfur-containing non-quenched and tempered steel via the EAF-LF-VD-CC route, performing early deoxidation in the LF and maintaining an MI below 0.15 improves sulfur yield. This avoids excessive desulfurization during LF and eliminates the need for sulfur re-addition during the VD process.

(2) Following rapid deoxidation, finely dispersed Al2O3 provides nucleation cores for MnS. Without massive sulfur additions, MnS inclusion size remains controlled, leading to a superior distribution of fine inclusions and enhanced steel quality.

Tip for Engineers: When operating with low MI slag (high SiO2 Or Al2O3), the slag becomes more aggressive. Ensure your Ladle Slag Line is protected with premium Magnesia Carbon Bricks to prevent premature lining erosion.

It is a precision slag control technique used to maintain high sulfur levels for machinability while achieving thorough deoxidation and steel cleanliness.
The MI represents the slag’s chemistry. For sulfur-containing steel, maintaining an MI around 0.15 suppresses desulfurization, ensuring a stable sulfur yield.

NEV steels require high strength and fatigue resistance, necessitating extremely low oxygen levels and minimal, finely dispersed oxide inclusions.

Comprehensive solution of Refractory for steelmaking