Since external air bricks are rarely used on 210t ladle, and are rarely used in domestic steel plants above 200t level, there is relatively little experience to learn from. According to the use experience, the following situations need to be paid attention to.
Failure to pull the porous plug brick core during hot replacement, and the replacement operation time is extended
The use conditions of the air brick core. When using a special air brick core pulling tool to pull the external air brick core, if the operation is improper, the outer iron sheet of the air brick core will be pulled off, and part of the air brick core will be retained in the seat brick, and it will have to be removed from the outside of the ladle using tools such as pneumatic picks, resulting in a bottom blowing replacement operation time of more than 3 hours.
Damage to the air seat brick caused by purging operation
When hot repairing the ladle, the air brick core is purged and cleaned, which will cause the air brick core to corrode faster than the air seat brick and sink into the seat brick. After the air seat brick loses its dependence on the air brick core, the inner cavity of the air seat brick is in direct contact with the molten steel. During use, it is subjected to the thermal shock of repeated circulation of molten steel, and the air seat brick is prone to breakage, causing the safety hazard of steel leakage due to drilling at the bottom of the ladle. At the same time, the blown-in Ar gas flows away from the fracture, which weakens the bottom blowing effect and affects the normal process treatment.

The life of the air brick core does not match the scheduled maintenance mode of the ladle, resulting in increased consumption of the porous plug brick core
The maintenance mode of the 210t carbon-free ladle is: 48 furnaces ~ 72 furnaces ~ 96 furnaces ~ 120 furnaces, that is, the ladle bottom bricks are replaced when the ladle age is 48 furnaces, the slag line bricks are replaced when the ladle age is 72 furnaces, the ladle bottom bricks are replaced when the ladle age is 96 furnaces, and the ladle bottom bricks are taken offline for repair at 120 furnaces. Since the service life of the air brick core after hot replacement is shorter than that of the air brick core installed on the new ladle bottom, when the ladle bottom life is set at 48 times, each air seat brick uses an average of ≥3 air brick cores, resulting in a large amount of air brick core usage, and the efficiency of the external air brick technology has not been fully utilized. Through the statistics of the service life and residual thickness of a large number of breathable brick cores on site (see Table 1), it is found that the service life of the breathable brick core installed on the bottom of the new masonry ladle is relatively long, while the service life of the breathable brick core after hot replacement is relatively short, which has a certain impact on the overall turnover of the ladle; at the same time, it also increases the consumption of breathable brick cores. The average consumption of breathable brick cores per bag is more than 14, and the highest consumption reaches 18.
| Bottom blowing statusHot change | Air brick core life/times | Remaining thickness/mm | ||||
| Maximum | Minimum | Average | Maximum | Minimum | Average | |
| Dumping | 15.2 | 21 | 11 | 213 | 300 | 180 |
| New installation | 10.4 | 24 | 2 | 265 | 350 | 210 |
| Bottom blowing status | 21.3 | 26 | 17 | 210 | 230 | 180 |
Misjudgment of the purge of the porous plug brick core affects the bottom blowing effect
Due to the stability of the production quality of the air brick core and the impact of the on-site purge operation of the air brick core, the air permeability of the air brick core will be insufficient when the ladle enters the refining station for processing, which is difficult to meet the requirements of the refining process. The molten steel has to be poured into another ladle for further processing, which has a certain impact on the normal production rhythm and increases the production cost.
Improvement measures and effects
In view of the failure of the air brick core to be pulled out during hot replacement and the long replacement operation time, it is required to fully purge the residual steel and residue bonded to the surface of the air brick core when replacing the air brick core, and at the same time, completely remove the fire mud bonded to the back seat of the air brick core; knock the air brick core before pulling, and at the same time improve the strength of the steel shell at the bottom of the air brick core, so that the pulling success rate and efficiency when replacing the bottom blowing are significantly improved.
For the purging operation of bottom-blown bricks, the purging operation specification of air-permeable bricks has been formulated, and clear requirements have been made for the purging gas flow, purging angle, purging time, etc., to improve the operator’s ability to judge the fracture and blockage of bottom-blown bricks.
Measures to match the life of air-permeable bricks with maintenance. For the local pits that appear in the core of the air-permeable bricks during use, timely repairs are made by adding repair materials to ensure that the air-permeable bricks operate in a safe state.
In response to the problems that arise during the use of on-site air-permeable bricks, the “Management Requirements for the Use of Air-Permeable Bricks” have been formulated to standardize the on-site management of suppliers and strengthen the communication and coordination between suppliers and operators at ladle preparation positions. Establish and refine dynamic records of the use and inspection of air-permeable bricks, promptly discover problems that occur in the use of air-permeable bricks, and quickly find corresponding solutions.
Through the improvement of the above technical measures and management methods, the current blowing rate of external air-permeable bricks has reached more than 99.9%, achieving a 100% success rate in the drawing of air-permeable brick cores, and greatly shortening the hot replacement time of air-permeable bricks. The service life of the porous plug brick core is stable at 24 to 28 times, and the residual thickness is greater than 200mm, which reduces the consumption of air bricks. The phenomenon of air seat brick fracture disappears, which greatly improves the safety of external air bricks. At the same time, in the past four years after the improvement, the service life of external air bricks has been well matched with the maintenance mode of ladle lining, laying the foundation for further improving the service life of ladle.