lmm@magnesiacarbonbricklmm.com

Technical support and construction service team

Mechanism of damage to the lining of the medium frequency furnace and design solutions to extend the service life of the lining

During the use of the medium frequency furnace, the thickness of the refractory material used for the lining is only 70-110mm. The inside is in contact with the high-temperature molten metal, and the outside is close to the water-cooling coil. The temperature difference between the inside and outside of the refractory material is large, and it is in a relatively thin section and a highly corrosive environment for many smelting operations. The main process conditions that affect the damage of the lining include: smelting temperature, degassing time, one-time degassing amount, chemical composition of the slag, and the type of steel (iron) produced. The main factors affecting the damage to the lining are: chemical erosion of the slag, spalling of the refractory structure, and thermal erosion.

Composition of the lining of the medium frequency furnace

The lining of the medium frequency furnace is usually made of refractory materials of various specifications and particle sizes (commonly used refractory materials are mainly magnesium, quartz, aluminum and composite materials). Its characteristics are: direct bonding. Therefore, it has high corrosion resistance, high mechanical strength, and good thermal shock resistance.

Mechanism of damage to intermediate frequency furnace lining

The damage mechanism of magnesium lining materials Taking magnesium refractory materials as an example, the damage mechanism of magnesium materials is explained: the main manifestations of magnesium material damage are: thermal erosion caused by flowing molten steel and chemical erosion caused by the penetration of slag components into the material. During the smelting process, the solution will penetrate into the refractory matrix through the capillary channels in the refractory matrix to corrode the lining. The components that penetrate into the refractory matrix include; CaO, SiO2, FeO in the slag; Fe, Si, Ai, Mn, C in the molten steel, and even metal vapor, CO gas, etc. These infiltrated components are deposited in the capillary channels of the refractory material, causing the discontinuity of the physical and chemical properties of the refractory working surface and the original refractory matrix. Cracks, peeling and loose structure will occur under the sudden change of operating temperature. Strictly speaking, this damage process is much more serious than the dissolution damage process.

The metal materials added to the furnace will bring in various oxides, and the slag components of different materials and different furnaces are also different. Most of the various oxides, carbides, sulfides and various forms of composite compounds in the slag will react chemically with the furnace lining to generate new compounds with different melting points. Some low-melting-point oxides such as iron olivine (FeOSiO2) and manganese olivine (MnOSiO2) generated in the reaction generally have a melting point of about 1200°C. Low-melting-point slag has excellent fluidity and may form a fluxing agent, causing severe chemical erosion on the furnace lining, thereby reducing the service life of the furnace lining.

The high-melting-point slag generated in the reaction, such as mullite (3Al2O3·2SiO2), forsterite (2MgO·SiO2), etc., and some high-melting-point metal elements have a melting point of more than 1800°C. There is also a relatively complex interpenetration and mutual dissolution between the high-melting-point slag and the low-melting-point slag suspended in the molten metal. These slags are very easy to adhere to the furnace wall and accumulate, causing serious slag sticking, affecting the power, melting speed and capacity of the electric furnace, and even affecting the life of the furnace lining.

As the furnace capacity increases, the proportion of heat lost from the surface of the molten steel decreases, the slag temperature is higher than that of a small-capacity furnace, and the fluidity of the slag is better than that of a small-capacity furnace, thus aggravating the erosion of the furnace lining. Large induction furnaces mostly use a mixed method of steel and slag to tap steel, which requires the slag to have good fluidity to adapt to the conditions of tapping. Therefore, the slag line is severely eroded, which is another reason for the reduction in the service life of the furnace lining. Due to the above reasons, the service life of the lining of a large induction furnace is lower than that of a small and medium-sized induction furnace. In order to increase the service life of the lining, the thickness of the lining should be appropriately increased. However, as the thickness of the lining wall increases, the resistance value increases, the reactive power loss increases, and the electrical efficiency decreases. Therefore, the thickness of the lining wall is limited to a certain range. Therefore, a reasonable wall thickness must be selected to ensure both high electrical efficiency and the service life of the lining.

Design of the solution

The above erosion leads to so-called structural spalling under cyclic temperature fluctuations. During the production process, molten slag penetrates into the pores of the refractory matrix, forming a large thickened refractory layer. The physical and chemical properties of the part of the refractory impregnated by the slag change. Due to the different thermal expansion coefficients between the penetration layer and the residual inconvenient layer, when the temperature changes, a large stress appears at the junction of the two layers, which leads to cracks parallel to the working surface and eventually causes spalling of the lining. The slag that penetrates into the refractory matrix dissolves the refractory particles and weakens the bond between the particles, resulting in a decrease in the material’s refractoriness and high temperature resistance. As a result, the refractory material in the slag penetration layer is damaged faster under the erosion of flowing molten steel.

The basicity of the slag should be adapted to the lining material. Magnesia lining materials can be corroded by high-CaO slag and SiO2 slag. The amount of CaF in the slag should be controlled. Excessive CaF will corrode the basic lining and cause premature melting of the slag line area. When the fluorine ions and metal manganese ions in the slag are high or the molten pool temperature is above 1700℃, the viscosity of the solution will also drop sharply, the damage rate of the furnace lining will accelerate, and the life of the furnace lining will be greatly reduced. When slag-free smelting is carried out under vacuum, the service life of the furnace lining is greater than that of non-vacuum smelting.

The infiltration of a high iron oxide content in the furnace lining destroys the microstructure of the original furnace lining, reduces the refractoriness, and reduces the viscosity of the CaO-Ai2O3-SiO2 slag, so that the slag penetrates deeper into the material. However, a certain amount of iron oxide in the original furnace lining is conducive to the rapid sintering of the furnace lining and reduces the open pores and air permeability of the material. In particular, when the molding material contains a certain amount of iron oxide, the rapid sintering of the material, the elimination of sand blasting and sand inclusion are very prominent.

Increasing the magnesium oxide content and the viscosity of the slag is beneficial to reducing the erosion of the slag on the furnace lining and improving the slag collection effect. When the slag basicity is low, the corrosion to the magnesia lining is more serious, and the life of the lining is reduced; on the contrary, when the slag basicity is high, the corrosion to the lining is relatively mild, and the life of the lining is relatively improved. Increasing the slag basicity and the MgO content in the slag and reducing the FeO content in the slag are beneficial to reduce the corrosion of the slag on the refractory material. Therefore, when using slag-making agents, attention should be paid to selecting materials with high magnesium oxide. Reasonably configure the slag structure, speed up the slag formation speed, shorten the smelting time, and reduce the iron oxide content in the slag.

The appropriate slag should be selected according to the material of the lining. Alkaline slag is suitable for magnesia lining, but it can be corroded by high CaO slag and SiO2 slag. Excessive CaF2 will also corrode the alkaline lining, causing premature melting of the slag line area. Acidic slag is suitable for quartz lining, and magnesia-alumina lining can only be suitable for weakly alkaline or neutral slag. Alumina furnace linings will show typical amphoteric properties at different pH values ​​at high temperatures. They can adapt to slags with different pH values, but they are slightly worse than acidic and alkaline linings. For this reason, some people use high-purity magnesia sand and add a certain amount of spinel to change the matrix properties of pure magnesia lining materials when selecting materials, but experiments show that the corrosion resistance of high-purity corundum materials is obviously inferior to that of sintered magnesia sand with low purity. Acidic slag is suitable for quartz furnace linings, while magnesia-alumina furnace linings can only be used for weakly alkaline or neutral slag. Alumina furnace linings will show typical amphoteric properties at different pH values ​​at high temperatures. They can adapt to slags with different pH values, but they are slightly worse than acidic and alkaline linings.

Conclusion

In conclusion, considering the main damage mechanism of magnesia furnace lining, after continuous summary and exploration, the material’s resistance to slag penetration can be improved by limiting the open pores and permeability, and the high-temperature erosion resistance and spalling resistance of the furnace lining matrix can be improved by increasing the high-temperature flexural strength and the critical softening temperature.

The performance of the furnace lining depends on many factors, such as the particle size distribution of the material, the physical and chemical properties of the material, and the sintering temperature of the furnace lining.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information