Methods of steel casting and refractory materials for steel casting
Molten steel is poured from a ladle into an ingot mold, either by top or bottom pouring, and is transported by flow bricks and intermediate containers of different uses (continuous pouring tundish, vacuum treatment chamber, refining ladle outside the furnace, etc.). The following complex and special-shaped products are used for steel casting: nozzle bricks, plug bricks, sleeve bricks, and seat bricks. These products are so-called interception devices, which are very important parts for steel casting. Recently, steel casting without interception devices is adopted – slide plates or sliding nozzles. If it is not continuous casting, in the process of steel casting, pouring bricks, funnel bricks, center pouring pipe bricks, center bricks, flow channel bricks and flow tail bricks are also used. The interception device with a stopper rod is maintained at the end by a stopper brick. The thick layer of molten steel in the ladle falls; although it is carefully separated by refractory sleeve bricks, it stays for a long time, especially in 350~450t ladles, and the stopper rod becomes soft under the overheating conditions of the molten steel. Among the refractory conditions of the cut-off device, the nozzle brick, plug brick and plug sleeve brick are very demanding, because the refractory is in the molten metal, and the plug brick is the most easily damaged. The second disadvantage of the cut-off device: the consumption of refractory is large: one set of sleeve bricks and plugs weighing 2~2.5kg are required to cast 1t of steel. The third disadvantage is that molten steel cannot be refined outside the furnace. So far, except for a few small and medium-sized steel mills in my country that use plugger cut-off devices, almost all use sliding nozzle devices, and with the increase of continuous casting ratio, steel bricks are gradually eliminated. The most complete plug-free casting requires a sliding nozzle that can slide. The working principle of the sliding nozzle: the molten steel must pass through two connected and perforated refractory accessories (slide plates, oil cylinders, etc.). This device is fastened to the bottom of the ladle from the outside, discharged by the upper nozzle, and completed from top to bottom by the second nozzle, usually the so-called lower nozzle, because its main function is to form a flowing stream of molten steel. The longitudinal section of the two slides and the sliding nozzle assembled and installed on the ladle is shown in the figure. The surface of the upper and lower slides to be installed should be polished with a grinding wheel or diamond. It should be pointed out that grinding itself brings considerable defects to the crystal surface of the refractory material. According to regulations: the gap between the slides should not exceed 25~50μm.

Sliding nozzle
The refractory material of sliding nozzle should have the following properties: high mechanical strength; low porosity when thermally stable; pore size should be less than 5μm; high refractoriness under load, low content of fusible impurities; the friction working surface cannot be wetted by metal. The sliding plate is mostly made of corundum, mullite corundum, carbon-bonded corundum and periclase. The type of refractory material for the sliding plate is determined by the grade and temperature of the pouring steel, the capacity of the ladle and the pouring method. Magnesium sliding plates have a relatively high service life for pouring low carbon steel (less than 0.1%℃) and high manganese steel. For ingot mold casting, when the number of streams is large, it is better to use corundum and mullite corundum sliding plates, although its corrosion stability is worse than that of magnesium sliding plates.

It is better to use magnesium slide plates for high temperature steel. To manufacture magnesium slide plates, fused periclase containing not less than 95% MgO and less iron oxide content, generally not more than 0.6%~0.8%, should be used. In order to improve thermal shock resistance, industrial alumina and other additives are added to the composition of the ingredients: the slide plates are formed at a pressure of 130~150MPa and fired at 1730℃. The slide plates are impregnated with phenolic plastic or tar pitch and heat treated. In some cases, they are impregnated and heat treated twice.
After impregnation and heat treatment, the slide plates have a porosity of less than 10% and a compressive strength of more than 80MPa. This slide plate is used in conjunction with unfired graphite magnesium upper and lower nozzles to withstand two turnover packages. The sliding nozzle refractory material lt steel consumes 0.2kg. The practice of some countries has concluded that the slide plates with corundum components and carbon combined (Al₂O₃77%, SiO₂8% and C11%). The characteristics of this slide are: its compressive strength is as high as 170MPa at room temperature, its flexural strength is 10.8MPa at 1400℃; its thermal expansion is about 1% at 1500℃; its elastic modulus is (63~53)×103MPa; its open porosity is 11%~15%; and its pore size is 2.8~0.4μm. China once used chrome corundum slides with good slag resistance, but now aluminum zirconium carbon slides are commonly used.

In order to make the sliding nozzle easy to open and close when pouring begins, a special mechanism is used to fill the ladle nozzle channel. For this purpose, dry magnesia powder, sand, a mixture of sand and graphite, a mixture of ash and graphite, kyanite-sillimanite and staurolite concentrates are used. The last two materials give better results. At the same time, before starting to pour steel, it is actually completely eliminated that the steel pouring channel must be flushed (burned through) with oxygen, which has a great corrosive effect on all accessories of the sliding nozzle. The metal condenses in the channel of the sliding device, and when the pouring is interrupted, the subcutaneous bubbles of the metal are prevented. A more reasonable way to solve the problem is to use porous annular air-permeable bricks, through which argon is blown.


