A steelmaking branch built and put into operation two 100t ladle refining furnaces in 1996, using a single column to control the three-electrode heating mode. The refining furnace uses three graphite electrodes to heat the molten steel. During heating, the three-phase electrodes are inserted into the slag layer and heated by submerged arc. At the same time, argon gas is stirred at the bottom of the ladle to form high-alkalinity reducing slag, which deoxidizes, desulfurizes, alloys, removes inclusions and other metallurgical reactions. This equipment is mainly used for heating and alloying molten steel, and plays a good connection role between the converter and the continuous casting machine. The consumption of graphite electrodes per ton of steel is one of the important indicators of refining production costs. In the actual smelting process, the annual consumption of graphite electrodes accounts for 15% to 20% of the total refining cost. Graphite electrodes are heated by submerged arc. In addition to being corroded by molten steel and slag, graphite electrodes will occasionally break, peel off joints, lack of blocks at the bottom of the electrode, and wrong buckles, which will increase the consumption of electrodes. The price of graphite electrodes has been running at a high level in recent years, which not only increases the smelting cost, but also affects the smooth production on site. In order to ensure the smooth operation of refining furnace equipment, accurately control the composition of molten steel, temperature hit rate and product quality, and effectively control costs, it is necessary to optimize and improve the production process and the use of electrodes. Reduce the consumption of electrodes per ton of steel, reduce the number of on-site electrode adjustments, reduce the labor intensity of workers, ensure the stable and smooth smelting of the refining furnace, achieve cost reduction and efficiency improvement, and also create conditions for the green and low-carbon development of enterprises.
Electrode consumption mechanism in the refining process
Graphite electrode is a conductive material made of artificial graphite. It uses petroleum coke and asphalt coke as aggregates and coal tar as a binder. It is made through multiple processes. Graphite electrodes have good conductivity and oxidation resistance, and form high-temperature arcs above 2000℃ on the surface of molten steel to transfer heat to the molten steel. During the heating process, argon is continuously blown from the bottom of the ladle, and the heat from the high temperature area on the surface of the molten steel is continuously brought to the low temperature area by the flowing molten steel, so that the entire furnace of molten steel continuously absorbs the heat from the high temperature arc, thereby increasing the temperature of the entire furnace of steel. Electrode consumption mainly includes electrode cut surface consumption, side consumption, and fracture consumption.
1.1 Consumption of electrode cut surface
Because a high-temperature arc is generated during the heating process, the electrode at the heating end sublimates at high temperature, and the end face of the electrode is consumed. Under the action of thermal stress, the end face of the electrode cracks or even falls off. At the same time, the erosion of the electrode by slag and molten steel will also cause chemical reactions or melting of the electrode. The different temperatures of the different parts of the end face of the electrode will produce thermal stress, which will also cause cracks and fractures in the electrode. This phenomenon will continue to expand with the increase of current intensity. The refining furnace is powered by high current and low voltage, and its arc length is short. The arc is easy to deviate outward under the influence of the electromagnetic effect of high current. The electrode will also be eroded by slag under the rolling and scouring of foamy slag. The molten steel level fluctuates under the stirring of argon gas at the bottom of the ladle, and the molten steel on the liquid surface scours the electrode, which will also cause the electrode to melt and consume, as shown in Figure 1. In the early stage of the refining process of molten steel, the slag is not reduced and has strong oxidizing properties. When the electrode contacts the oxidizing slag, the iron oxide, manganese oxide and other substances in the slag react with the electrode chemically. In the later stage of refining and smelting, the slag reacts with the carbon element contained in the electrode, which also causes the electrode to melt and consume. Therefore, argon blowing at the bottom of the ladle, process temperature control, and target control of molten steel composition will affect the consumption of graphite electrodes.

Figure 1 Electrode end surface consumption diagram
1.2 Electrode side consumption
The side consumption of the electrode refers to the oxidation consumption of the cylindrical surface of the electrode. Under normal circumstances, the furnace is slightly negative pressure, and the surface of the graphite electrode reacts chemically with the oxygen in the furnace gas. When the graphite electrode exceeds 400℃, oxygen easily reacts with the surface of the graphite electrode. When the temperature reaches above 600℃, the oxidation reaction becomes more intense, as shown in Figure 2. This reaction is very sensitive to the air flow velocity and oxygen concentration on the surface of the graphite electrode. When the oxygen pressure in the refining furnace is low, the side consumption of the electrode is relatively small. During the refining and smelting process, the oxidation reaction of carbon is relatively weaker than the gasification reaction of carbon, so it is not the main reason for the consumption of graphite electrodes.

Figure 2 Electrode side consumption
1.3 Electrode breakage consumption
Electrode breakage usually occurs at the joint between the first and second electrodes, as shown in Figure 3. The main reason is that the degree of rotation is not enough when the electrodes are connected, resulting in looseness or the dust at the connection between the two electrodes is not cleaned up, and there is a small gap, which leads to an increase in the resistance between the electrodes, and the connection is prone to local overheating and reddening. The front end of the electrode is oxidized and eroded to become thinner. During the temperature rise process, it is also affected by electromagnetic force; the single column controls the heating mode of the three electrodes, causing the electrode lifting system to operate unstably, which easily leads to high-position breakage of the electrode, which often occurs after adjusting the electrode for 3 furnaces of steel, forcing the refining and smelting to be terminated.

Figure 3 Electrode high position fracture diagram
Measures to reduce the consumption of graphite electrodes in refining furnaces
2.1 Select reasonable power supply parameters and systems
(1) The power supply system of the refining furnace in the steelmaking plant is divided into 10 gears. Within the voltage range of 200-300V, different gears have different heating powers and different heating speeds. Optimize the power supply power, use reasonable voltage and current gears, maintain the stability of the arc, and reduce the impact of electromagnetic induction. Optimize the power supply process according to the steel smelting cycle, and determine that the refining furnace should use gears 1-4 for slagging, 7-9 for heating, and 4-7 for insulation.
(2) Optimize the power supply system. The melting loss of the electrode end surface is proportional to the current intensity and heating time, and the relationship is as follows:

Where: Ctip is the melting loss at the lower end of the electrode, kg/t; Rsub is the sublimation rate, kg/(kA²·h); I is the current, kA; Tpo is the power-on heating time, h; P is the refining furnace productivity, t/furnace. According to the above formula, combined with the refining and smelting characteristics of the steelmaking plant, the power supply heating mode is optimized according to the conditions of molten steel and slag. In the early stage of molten steel refining, short arc and high power gear heating are used to quickly melt the slag; after the slag is melted, a long arc is used to increase the power and increase the heating speed; in the later stage of molten steel refining, the appropriate arc length and input power are selected to accurately control the molten steel temperature within a certain range and reduce the consumption of the electrode section and side.
2.2 Formulate a reasonable slag making system
(1) Addition and proportion of slag. It has been observed that the arc length is 70-90mm during heating and power transmission, so the thickness of the slag layer should be controlled at no less than 100mm. Through calculation and actual operation, it is concluded that the weight of slag brought into the ladle should be controlled at 700-1200kg, mainly including lime, deoxidizer, calcium carbide, etc. (2) When heating the electrode, the slag should be added in batches in small amounts and multiple batches to prevent excessive slag from being added into the ladle at one time to form a lump of material, and to avoid collision between the electrode and the lump of material causing electrode damage. (3) Create an alkaline reducing atmosphere as soon as possible to form micro-foamed refined white slag as soon as possible to reduce the impact of the oxidizing environment on the electrode. (4) Establish a reasonable slag return system, that is, the reuse of refined white slag. Refined white slag is an alkaline reducing slag. Refined white slag is added to the newly treated molten steel by front or back return, and argon stirring and deoxidizer are added to produce alkaline reducing slag more quickly. After the furnace with slag return, the slag is relatively easier to melt when the refining furnace is powered on and heated at the initial stage, and the initial slag melting time is significantly shortened. In addition, the refined white slag has good foaming properties, which is conducive to the early submerged arc heating of the graphite electrode, improving the efficiency of electric energy utilization and reducing the refining heating power supply time. By returning slag, the power supply time of a single furnace and the refining power consumption can be reduced, and the high-position breakage of the steel electrode in the 3 furnaces after adjusting the electrode can be effectively avoided.
2.3 Reasonable temperature control throughout the process
Timely hot repair of the ladle to ensure that the hot ladle is in place to avoid the phenomenon of the converter waiting for the ladle. When smelting low-phosphorus and low-sulfur steel, make full use of the scrap steel baking furnace and preheat the ladle for 8 to 10 minutes, so that the ladle can be preheated from 1000°C to 1200°C, maintain the ladle temperature and enhance the heat storage capacity of the ladle, effectively ensure that the low-phosphorus and low-sulfur molten steel reaches the refining temperature, and ensure that the refining treatment time is reduced as much as possible under the condition of smooth continuous casting, shorten the refining heating time, and reasonably control the converter tapping time and temperature, strictly control overoxidation tapping, implement the contact system for the converter, refining and continuous casting processes, grasp the production sequence, and create good conditions for achieving just-in-time production.
2.4 Reasonable control of argon stirring
Reasonably control the flow rate and intensity of argon stirring to avoid molten steel flushing the electrode and causing electrode consumption. Argon stirring is carried out throughout the refining and smelting process, and the argon flow rate needs to be dynamically controlled in stages. By reasonably controlling the argon flow rate, the slag sticking on the furnace cover can be reduced, and the electrode breakage accident caused by the strong flow of molten steel can be avoided. The steelmaking plant conducted data statistics and analysis on the argon regulation and molten steel flow field during the refining bottom blowing process and found that different molten steel conditions have a greater impact on the argon blowing effect. Based on the comprehensive analysis of the test data and the inspection results, the optimal parameter standard for argon flow control of the refining bottom blowing is determined, as shown in Table 1.
| Stage | Time/min | Flow rate range/(L·min-¹) | Main purpose |
| Breaking the top stage | 0.1~0.2 | 500~600 | Use high pressure and large flow argon to stir the molten steel and break the slag shell |
| Sampling stage | 1~2 | 30~60 | Use uniform molten steel composition and temperature, weak blowing to facilitate temperature measurement and sampling |
| Slagging stage | 3~6 | 100~260 | Quickly form refined slag with high basicity and low oxidizability |
| Tempering stage | 10~20 | 150~300 | According to the comprehensive consideration of molten steel in-situ temperature, various heat losses and heating rate, meet the requirements of steel grade out-of-situ temperature |
| Desulfurization stage | 2~5 | 400~500 | Use strong stirring to promote the migration of sulfur from molten steel to the steel-slag interface, chemical reaction occurs, and sulfide is generated to migrate to the slag layer |
| Fine-tuning stage | 1~3 | 150~200 | Finely adjust the alloy according to the in-situ composition to meet the requirements of the steel grade |
Table 1 Effect of bottom blowing argon flow control
2.5 Reasonable control of dust removal intensity and optimization of electrode wrench
(1) Reasonably control the operation intensity of dust removal equipment according to actual production conditions, and appropriately reduce the operation intensity of dust removal equipment while ensuring the dust removal effect. Change the opening degree of the dust collector valve according to different stages of smelting to control the air to be sucked into the ladle as little as possible. Through bottom blowing argon, submerged arc heating, deoxidation, and lifting of the furnace cover, the reducing atmosphere of the ladle is ensured, and a micro-negative pressure is formed in the ladle to avoid oxidation reaction between oxygen in the air and the graphite electrode. (2) Optimization of electrode wrench. Graphite electrodes are weak in strength and easy to break. The graphite electrodes used in the actual smelting process are long electrodes connected by short electrodes. Therefore, the connection quality and tightness of the graphite electrode are crucial. Eliminate wrenches with excessive or insufficient torque. According to the actual situation on site, optimize the electrode torque parameters to ensure the connection quality. When the torque value reaches the specified ideal value during use, the wrench will make a sound, and the wrench will be partially unloaded, ensuring the connection quality of the graphite electrode. In addition, the electrode must be purged clean when connected, and the electrode must be rotated in place to avoid micro gaps at the joints of the electrode, which can effectively prevent the electrode from breaking at a high position.
Conclusion
Through the exploration of reducing the consumption of ton steel of electrodes in the refining furnace, the phenomena of molten steel scouring the electrode, electrode oxidation and peeling, and accidental electrode breakage have been significantly reduced, and the consumption of ton steel of the electrode has been significantly reduced, from the average electrode consumption of 0.544kg/t in 2021 to the current 0.347kg/t. It ensures the stable operation of the refining equipment, improves the output and quality of steel billets, and effectively reduces the occurrence of production accidents and the labor intensity of operators.