Abstract: In view of the current situation that the lining of the double-nozzle fully refined ladle is seriously eroded, affecting the safe use of the ladle and restricting the smooth production, the life improvement of the double-nozzle fully refined ladle is studied. By developing and applying technical means such as composite masonry of the ladle lining, refining powder spraying slag adjustment, and electrode splashing slag filling, the life of the double-nozzle fully refined ladle is greatly improved, and the ladle life is increased from 35.9 times to 53.7 times.
1 Introduction
The steelmaking plant of a certain company currently has two 10-machine 10-stream small square billet continuous casting machine production lines, using a double tundish casting mode. In order to meet the production requirements of furnace machine matching, a double-nozzle double-air-permeable brick ladle design is selected. In the early stage of production, affected by production organization, converter operation, refining process, etc., the pouring temperature of the continuous casting process was high, resulting in high refining outlet temperature, poor converter endpoint control, low endpoint carbon, many molten steel peroxidation heats, and serious erosion of the ladle lining; in addition, due to equipment failure, the continuous casting process was abnormally shut down, resulting in the molten steel staying in the ladle for a long time, seriously reducing the service life of the ladle.
Due to the serious erosion of the ladle lining, bricks fall off from the slag line from time to time, the ladle shell turns red, and the hidden danger of piercing is great, which has affected the safe use of the ladle and restricted the stable and smooth production. How to improve the safety operation coefficient of the ladle under full LF refining conditions, and study the life improvement of the double-sprue full refining ladle.
2 Factors affecting the life of the ladle
The initial function of the ladle is to receive the molten steel smelted in the converter or electric furnace, and transport the molten steel to the refining process for processing or the continuous casting process for pouring. With the development of steelmaking technology, the ladle, as a container for the secondary smelting reaction of molten steel, has added the following functions: heating, vacuum degassing (dehydrogenation, deoxidation) and removal of inclusions; alloying, uniform composition and temperature; slag making (desulfurization) and other functions. With the advancement of refining technology outside the furnace, the requirements for the material and life of the ladle lining are becoming more and more stringent. At present, the ladle lining of the branch steelmaking plant is designed as a composite masonry ladle, and magnesia carbon bricks are used for masonry at the slag line, because magnesia carbon bricks perform stably and well in terms of performance requirements such as refractoriness, corrosion resistance and thermal shock resistance. By observing the condition of the ladle offline, obvious erosion occurred in the slag line of the ladle and the impact zone of the ladle bottom, and the erosion at the slag line was the most serious, which had the greatest impact on the life of the ladle.
2.1 Erosion analysis of slag line magnesia carbon bricks
Many scholars have conducted in-depth research on the damage mechanism of slag line magnesia carbon bricks, and concluded that the erosion process of magnesia carbon bricks is: oxidation → decarburization → loosening → erosion → scouring → shedding → damage. During the refining process of the ladle, the carbon contained in the slag line magnesia carbon bricks reacts with the iron oxide and magnesium oxide in the slag at high temperature to form a decarburization layer on the surface of the magnesia carbon bricks. Due to the oxidation and removal of carbon, the internal network structure of the magnesia carbon bricks is destroyed, making the brick body loose and brittle, and the erosion is aggravated under the scouring of molten steel. At the same time, due to the loose structure of the brick body, the slag penetrates into the interior through the decarburization layer and reacts with the magnesia sand particles, causing the magnesia carbon bricks to be continuously oxidized and decomposed from the inside to the outside, accompanied by structural peeling, and then washed away by the steel slag, gradually eroding and thinning the brick layer.
2.2 Erosion analysis of the bottom of the ladle
Due to the high temperature of the molten steel, the high power of the refining power, and the strong stirring during the process, the scouring of the refractory material lining the ladle is more serious. In particular, the working layer of the ladle bottom has the longest contact time with the high-temperature molten steel, bears the greatest static pressure of the molten steel, and has a worse working environment. The ladle bottom is made of knotted castables. As the age of the ladle increases, pits appear in the impact area of the ladle bottom due to erosion by the molten steel, which poses a great safety hazard and affects the pouring utilization rate of the molten steel.
2.3 Slag basicity
During the refining process, when the amount of lime added is small, the slag basicity will be low and weakly acidic. Magnesium carbon bricks are alkaline refractory materials, and the two are prone to chemical reactions under high temperature conditions, causing the decomposition of magnesium carbon bricks. The alkalinity decreases, the slag becomes thinner, and the erosion of the ladle slag line is aggravated during the bottom blowing and stirring process. CaO and SiO2 in the slag enter the periclase grains through the decarburization layer, react with MgO, and generate low-melting point compounds such as CMS and C2MS3. Under the action of these low-melting point compounds, the periclase grains enter the slag, causing the magnesia carbon brick body structure to be loose and gradually melt loss occurs.
2.4 Refining process control
Due to the influence of production rhythm, the refining cycle of most furnaces is too short and the slag is not good. In addition, there is a lack of practical experience in the use of ultra-high power electrodes. The pursuit of high voltage and high power for rapid temperature increase leads to poor arc burial effect. The arc flow directly acts on the magnesia carbon bricks, causing obvious erosion of the slag line of the ladle, and bricks falling off the slag line from time to time. The observation of the ladle condition of the previous offline ladle showed that there were many holes on the magnesia carbon bricks on the slag line of the ladle wall. After analysis, it was due to the fact that the slag could not bury the arc or the arc burial effect was poor during the refining power-on process, and the arc light and heat radiation.
3 Key technology development and application
3.1 Composite masonry technology for ladle lining
Based on the erosion conditions in different areas of the ladle, the composite masonry structure of the ladle lining is reasonably designed: for areas with severe slag line erosion, replace the slag line magnesia carbon bricks with fused magnesia and large crystalline magnesia as the main raw materials; for the situation where the impact zone at the bottom of the ladle is eroded and pitted, add a “steel platform” at the impact zone; for the situation where the ladle mouth material is not resistant to erosion, use corundum material to seal the ladle edge (see Figure 1).

Two masonry methods were selected for the slag line where the erosion was the most serious: ① The high-alumina castable in the permanent layer slag line was replaced with corundum castable. Due to the more erosion-resistant characteristics of corundum, even if the slag line magnesia carbon bricks were eroded, there would be no danger of piercing the ladle. ② Double slag line bricks were used for composite masonry in the slag line. When the working layer magnesia carbon bricks were eroded and fell off, there was still a safety layer of magnesia carbon bricks, which was conducive to the timely judgment of the ladle inspectors.
3.2 Refining powder spraying slag adjustment technology
By spraying dolomite powder and coke powder, the slag composition and oxidizability of the refining and smelting process were improved, and the erosion of the slag lining by the refining process slag was reduced. A ring-shaped powder spraying device is added to the refining furnace cover (see Figure 2). The powder spraying device is a ring-shaped hollow steel pipe, which is installed below the refining furnace cover, 300 mm away from the outside of the furnace cover. There are several spraying holes with a diameter of 15 mm on the opposite side of the ladle. The angle between the center line of the spraying hole and the vertical line is 15° to the center of the furnace cover. This angle can effectively spray the powder to the slag surface 50-100 mm outside the electrode during spraying, so that the powder and slag can be quickly integrated to improve the slag composition and oxidizability.

After the converter is finished tapping and the ladle enters the station, the dolomite powder surface injection model of the refining process is selected according to the converter final slag index and slag volume. The injection model mainly determines the amount of dolomite powder surface and coke powder injection based on the converter final slag index and the amount of slag in the ladle after tapping. After injection, the slag composition and oxidizability in the ladle (MgO and FeO in the slag) can ensure the refining effect while slowing down the erosion of the ladle lining.
3.3 Electrode slag splashing ladle filling technology
Based on the principle of converter slag splashing furnace protection technology, the terminal slag with saturated or supersaturated MgO content is splashed onto the ladle wall through the action of the electrode arc flow. Through the subsequent ladle operation process, the slag is cooled and solidified, and a layer of high melting point slag layer is formed on the surface of the ladle lining, and it is well bonded to the ladle wall lining. The splashed slag layer has good corrosion resistance, and can inhibit the oxidation and decarburization of the slag line brick surface, and reduce the erosion and scouring of the slag line brick by high-temperature slag, thereby protecting the ladle lining and improving the service life of the ladle.
Referring to the CaO, Al2O3, SiO2 ternary slag phase diagram and according to the actual test results of the slag on site, it is required that the magnesium oxide content in the slag must reach more than 8%, and the slag must have a certain fluidity and viscosity. The slag is too thin to splash, and the slag is too viscous to adhere well. When the temperature and composition of the molten steel meet the requirements and are ready for soft blowing and exit, adjust the bottom blowing gas source flow to keep the liquid level stable, select low voltage and high arc flow for short arc operation, splash the slag onto the ladle lining, form a slag layer of a certain thickness on the ladle lining, and extend the service life of the ladle lining.
4 Application effects
(1) The service life of the double-nozzle fully refined ladle is greatly improved. The primary ladle age has increased from 35.9 times to 53.7 times, the residual thickness of the slag line bricks meets the requirements for safe use, and the safe operation coefficient of the ladle has been significantly improved.
(2) Baking gas consumption is significantly reduced. After the service life of the ladle is increased, the frequency of the ladle being put on and off the line is greatly reduced. Before the project was implemented, the consumption of gas for drying the ladle was 25m3/t, and is currently around 15m3/t.
(3) The large bag injection margin is significantly reduced. Due to the reasonable design of the ladle lining masonry structure, the bottom of the ladle on the nozzle side is lower than the breathable brick side, which facilitates the flow of steel and reduces the situation of steel leaving the pit at the bottom of the ladle. Before the implementation of the project, the bale injection margin was basically around 350 kg/furnace, and is currently controlled at around 220 kg/furnace.
(4) The converter tapping temperature is effectively reduced. The life of the ladle is increased, abnormal ladle input is reduced, the red envelope turnover rate is increased, and the process temperature drop is reduced.