Converter furnace lining
As the core equipment for steelmaking, the quality of converter furnace lining construction directly determines the service life and production efficiency of the converter. This scheme combines advanced domestic and foreign experience to build a systematic solution from three dimensions: material selection, process optimization, and quality control. Focusing on the differences in working conditions in different parts, it proposes a full-process technical system of “zoning material selection + precise construction + dynamic maintenance”.

01 Material system and performance adaptation
(I) Working layer material selection
Magnesium carbon brick system
Slag line area: MT18A magnesia carbon brick (MgO ≥ 88%, C ≥ 14%) is used. Its slag erosion resistance index is 35% higher than that of ordinary magnesium carbon bricks, and it is suitable for areas with slag erosion rate > 2mm/furnace.
Charging side: Anti-oxidation magnesium carbon bricks with 0.5% metal aluminum powder added are used. After 1600℃×3h thermal shock test, the residual strength retention rate reaches 82%.
Steel outlet: equipped with integrally cast magnesium carbon casing bricks, the inner diameter tolerance is controlled within ±0.5mm, and high-aluminum ramming material is filled to ensure no leakage for more than 2000 thermal cycles.
Application of amorphous materials
The annular area of the furnace cap adopts Al₂O₃-MgO self-flowing castable material, the construction fluidity is ≥220mm, and the volume density reaches 2.95g/cm³ after drying at 110℃×24h.
The permeable bricks are filled with corundum quick-drying anti-seepage material, the penetration depth is ≤1mm/24h, which effectively blocks the penetration channel of molten steel.
(II) Optimization of permanent layer materials
The fired magnesium bricks use fused magnesia aggregate (MgO≥97%), the apparent porosity is ≤16%, and the linear change rate after firing at 1550℃×3h is only -0.12%.
A 5mm thick Helu ceramic fiber paper expansion joint is set between the permanent layer and the working layer, and the compensation coefficient is 0.8%/1000℃ to avoid thermal stress concentration.
02 Standardized construction process
(I) Construction preparation
Environmental control
A temperature and humidity monitoring system is set up in the masonry area. Construction can only be carried out when the ambient temperature is greater than 5℃ and the relative humidity is less than 70%.
Refractory bricks need to be preheated at 200℃×24h, and the moisture content is ≤0.3%.
Equipment calibration
A laser rangefinder is used to locate the center of the furnace body, with an error of ≤±1mm.
The amplitude of the vibrating rod is controlled at 0.5±0.05mm, and the frequency is 12000 times/min, ensuring that the density of the ramming material is ≥2.8g/cm³.
(II) Partial masonry technology
Furnace bottom construction
The permanent layer is masonry using the “cross method”, and the upper and lower layers of magnesium bricks are staggered at 90°, and the thickness of the mortar joint is ≤1mm.
A laser centering system is used when installing air-permeable bricks, with a positioning accuracy of ±0.2mm, and silicon carbide sealing material is filled around the tail pipe.
Furnace body construction
The working layer implements the “spiral rising method”, each ring door brick is displaced ≥3 pieces, the expansion joint is arranged according to “three horizontal and four vertical”, and the spacing is controlled at 1.2-1.5m.
The ear axis part adopts prestressed anchoring technology, a dovetail groove is opened on the surface of the refractory brick, and a 310S stainless steel anchor with a diameter of 8mm is implanted.
Furnace cap construction
Use an adjustable arc template to ensure that the roundness error of the cone part is ≤3mm/m.
The furnace mouth brick pressing material uses magnesium dry vibrating material, which is rammed in three layers, and the compaction coefficient of each layer is ≥0.95.
(III) Key node control
Transition zone treatment
The transition section between the molten pool and the furnace bottom arc uses customized special-shaped bricks, and the curvature radius deviation is ≤±2mm.
A 2mm thick phosphate binder is applied between the permanent layer and the working layer to form a transition bonding layer.
Optimization of baking furnace curve
The “three-stage heating method” is adopted:
Low temperature section (room temperature-300℃): heating rate ≤15℃/h, constant temperature for 8h to remove free water;
Medium temperature section (300-800℃): heating rate ≤25℃/h, constant temperature for 12h to complete the decomposition of crystal water;
High temperature section (800-1200℃): heating rate ≤35℃/h, constant temperature for 24h to achieve sintering densification.
03 Quality Control System
(I) Process Monitoring
Infrared Thermal Imaging Detection
After each layer of masonry is completed, the surface temperature is scanned. Areas with a temperature difference of >15°C require local rework.
The furnace shell temperature is monitored in real time during the furnace baking process, and the emergency cooling system is activated when the local hot spot is >250°C.
Ultrasonic flaw detection
Sampling of key parts (air-permeable bricks, steel outlets) is performed, and it is judged as unqualified when the defect equivalent diameter is >φ3mm.
(II) Acceptance Standards
Dimensional Accuracy
The verticality deviation of the furnace body is ≤5mm/m, and the total height error is ≤15mm.
The width deviation of the expansion joint is ≤±1mm, and the straightness error is ≤2mm/m.
Physical and Chemical Indicators
The apparent porosity of the working layer is ≤18%, and the compressive strength is ≥80MPa (1400℃×3h).
The load softening temperature of the permanent layer is ≥1650℃ (0.2MPa).
04 Innovative technology application
3D printing prefabricated parts
For complex structures (such as breathable brick bases), Al₂O₃-ZrO₂-C quality printed parts are used, with a dimensional accuracy of ±0.1mm and a 40% increase in installation efficiency.
Intelligent temperature control system
The embedded optical fiber sensor monitors the temperature gradient in real time and automatically adjusts the heating power when ΔT>50℃/h.
Nano modification technology
Adding 0.3% nano-SiO₂ to the castable increases the thermal shock parameter (TSP) from 250 times to 400 times (1100℃ water cooling).
05 Converter baking solution
After putting firewood and coke into the converter, heat it up for 5 to 8 hours. When the temperature rises to 1200-1300℃, molten iron can be added for trial burning. When smelting the first batch of steel, all molten iron must be added, and scrap steel is not allowed.
06 Furnace type optimization
Based on CFD simulation, the thickness distribution of the furnace lining is adjusted to increase the thickness of the slag line area by 15% compared with the traditional design, and reduce the thickness of the trunnion area by 10%.
This solution extends the life of the converter furnace lining to more than 8,000 heats through the collaborative innovation of materials, processes and maintenance, reduces the consumption of refractory materials per ton of steel to 0.8kg/t, and reduces the comprehensive maintenance cost by 35%. In actual application, dynamic adjustment is required in combination with specific furnace parameters. It is recommended to conduct laser scanning detection every 50 heats and establish a three-dimensional digital twin model to guide precise maintenance.
What are the key preparation steps required before starting the converter masonry process?
Before laying any bricks, a thorough inspection and preparation phase is essential. This includes:
Cleaning the furnace shell: Removing all residual slag and old refractory materials to ensure a smooth surface.
Checking the mechanical parts: Ensuring the furnace tilting mechanism and cooling systems are functional.
Tool and material readiness: Verifying that the magnesia carbon bricks are dry and undamaged, and that specialized masonry equipment (like brick-laying machines or lifting platforms) is calibrated.
Safety checks: Implementing strict ventilation and lighting protocols for workers entering the confined space.
Why is the “staggered joint” (overlapping) method used during brick laying?
Staggered jointing is a standard requirement for converter linings to prevent “straight-through seams.” If joints are aligned vertically, molten steel or slag can easily penetrate the gaps, leading to rapid erosion or even the “floating” of bricks. Staggered joints create a zigzag path that significantly reduces the risk of steel penetration and improves the overall structural integrity of the lining against the mechanical stress of furnace tilting.
Which areas of the converter lining require special reinforcement or thicker masonry?
The converter experiences uneven wear, so a “balanced lining” (zonal lining) approach is used:
The Charging Side: Reinforced to withstand the physical impact of scrap steel and the erosion of molten iron being poured in.
The Tapping Hole: Subjected to high-velocity molten steel flow and severe oxidation; usually constructed with specialized taphole blocks.
The Trunnion Areas: These are difficult to repair during operation, so higher-grade, erosion-resistant magnesia carbon bricks are typically used here.
The Slag Line: Specifically reinforced to resist chemical attack from aggressive furnace slag.
How are expansion joints managed in magnesia carbon brick masonry?
Magnesia carbon bricks have a high thermal expansion coefficient due to the magnesia, but the graphite content provides some degree of flexibility.
In many modern schemes, thin cardboard or specialized paper is placed between certain layers or sections to act as temporary expansion joints.
As the furnace heats up, these materials burn off, providing the necessary space for the bricks to expand without crushing each other or deforming the outer furnace shell.
Why is the “baking” (heating) curve critical after the masonry is completed?
Once the masonry is finished, the furnace cannot be used immediately. It must follow a strict heating-up schedule to:
Remove Moisture: Slowly evaporate any residual moisture in the ramming materials or mortar to prevent steam-induced explosions or cracking.
Carbonize the Binder: Allow the phenolic resin binder in the bricks to undergo proper polymerization and carbonization, which gives the bricks their final strength.
Prevent Thermal Shock: Gradually bring the refractory materials to operating temperature to avoid sudden stress fractures (spalling) caused by rapid temperature changes.