Ladle baking is a crucial step in steelmaking. Newly constructed ladles, cold-repaired ladles, drying ladles, and ladles undergoing turnover all require baking. A baking time curve is necessary before baking, and baking personnel must record the start time, baking time, temperature, and end time for each stage.
During the construction and pouring of the refractory bricks or castables lining the ladle, a certain amount of water is added. This results in a relatively high moisture content in the lining material after construction, requiring specific baking procedures based on the materials and baking regime. If shortcuts are taken or the correct baking method is not followed, it can lead to lining material peeling or thermal stress damage, ultimately affecting the ladle’s service life and, in severe cases, even its safe operation.
The purpose of baking is to remove free water and crystal water from the refractory lining after construction, allowing the high-temperature performance of the refractory material to be fully realized. The heating curve for baking is usually provided by the supplier of the refractory lining. If the project involves construction, the baking is typically carried out by the construction team before handover. The heating curve for baking a newly built steel ladle is usually divided into three stages, with a total time of 24 hours. The steel ladle should be baked at around 1100℃, or at least above 1000℃, until it stops smoking.
The first stage involves a low flame for 6 hours, without using a blower. The gas flame should be adjusted to the molten pool area of the ladle. During this process, the main purpose is to dry the moisture added to the refractory mortar and castable during the ladle’s construction, as well as the surface of the refractory bricks. Moisture in the lining will evaporate into water vapor at 110℃, resulting in rapid and large-scale dehydration. The discharged moisture has a significant impact on the castable and lining; therefore, the gas flame must not be too large, as this can easily cause the refractory material surface to crack.
The second stage typically lasts 8 hours. The gas flame should be adjusted to the bottom of the ladle, again without a blower. The temperature should rise slowly. A rapid temperature rise will cause the refractory material surface to dry too quickly, and the large amount of vaporized moisture that cannot escape will generate destructive steam pressure, causing cracks or fissures in the refractory material. During this stage, it is crucial to heat different parts of the ladle and different types of refractory materials simultaneously, while also drying the moisture in the castable at the bottom of the ladle.
The third stage, lasting 10 hours, involves adjusting the gas flame to the bottom of the ladle, then returning it to the slag line area. Simultaneously, the blower is turned on to convert the bound water and crystal water in the ladle into gas, which is then discharged through the vent. When the baking temperature reaches 600℃, the refractory material completes its crystal transformation and polymerization, forming an organic bond.
However, it’s important to note that prolonged baking can cause oxidation and decarburization of the lining material, affecting the service life of the ladle lining. We discussed this issue in yesterday’s article on ladle slag line damage; some ladles developed a decarburized layer of tens of millimeters on the magnesia-carbon brick layer during baking after construction. Therefore, it is recommended that newly constructed ladles undergo anti-oxidation coating treatment on the slag line area or beeswax board coverage during baking.
During the baking process, some manufacturers encounter problems such as the bursting of the castable refractory inside the ladle. The reasons for this are generally as follows:
1. Causes Related to Construction Quality: During construction, uneven mixing, excessive water addition, uneven distribution, and improper vibration time control can lead to voids in the castable refractory blank. Excessive or insufficient solidification of the castable during construction, decreased fluidity, and short construction time can also contribute to the problem.
2. Excessive Heating Rate During Baking: As mentioned earlier, the main purpose of baking the ladle is to remove free water and crystal water from the lining and to achieve optimal high-temperature performance of the refractory material. If operators do not strictly follow the baking curve during baking, arbitrarily adjust the gas or fan size, or allow for unstable fire intensity, it can lead to poor moisture removal from the lining, causing cracks in the ladle lining, and even resulting in lining peeling, cracking, or bursting.
3. Quality Issues with the Lining Castable: During the baking process, if the material’s strength is insufficient as the temperature rises, bursting can occur.
Simultaneously, during the baking process, all abnormal phenomena and problems that occur, along with the corresponding measures taken, should be documented for future reference and to learn from experience, serving as a basis for improving baking operations.
During baking, the condition of the inner lining should be carefully observed, monitored, and maintained to promptly identify any abnormalities and take appropriate measures to ensure smooth baking.
A strict shift handover system must be implemented, and all records during the baking process must be meticulously maintained.
A warning line should be established; unauthorized personnel are strictly prohibited from entering.