The converter generally needs to be repaired after 1000 furnaces and when the refractory lining has begun to damage. Repairing the converter is an important operation process to improve the converter life.
01 Repairing the large surface
Generally, the front and rear large surfaces (the front large surface is also called the front wall, and the rear large surface is also called the rear wall) are repaired crosswise. The operation steps are as follows:
(1) The viscosity of the final slag of the previous furnace for repairing the large surface should be slightly higher and not too thin. If the FeO content in the slag is too high and the furnace wall is too smooth, the repair charge will not easily stick to the furnace wall.
(2) After the previous furnace for repairing the large surface has tapped steel, the furnace shaker shakes the furnace so that the converter mouth is downward and the residual steel and slag in the furnace are poured out.
(3) Shake the furnace to the working position required for repairing the furnace.
(4) Pour the charge. According to the damage of the lining, pour 1~3t of filler material into the furnace (the specific amount depends on the size of the converter, the area and degree of the lining damage. The amount of filler material in the early stage of the furnace can be appropriately less), and then shake the furnace to spread the filler material evenly on the large surface that needs to be filled.
(5) Patching. The patching operation requires that the patches are arranged neatly, the brick joints are crossed, and the bricks are prevented from being missed or overlapped, so that the two sides and the joints are fully patched. Patching is generally not used in large converters.
(6) Baking. Let the furnace remain still and naturally bake the filler material based on the temperature of the molten pool in the furnace. The baking time is required to be 40-100 minutes. In the early stage of baking, it is best to insert two coal oxygen guns at the furnace mouth to blow oxygen to assist combustion, which is conducive to the sintering of the filler material.
02 Filling the furnace bottom
The key points of filling the furnace bottom are as follows:
(1) After adding the filling charge to the converter, first shake the converter to the rear large surface -30°, then shake the converter to the front large surface +20°, and finally shake the converter to 0°, ensuring that the sintering time is not less than 40 minutes. After the filling charge has adhered to the furnace bottom, slowly shake the furnace to the large surface position and continue sintering with the gas gun for 10 minutes. Before adding molten iron, first add 3-5 tons of molten iron into the furnace, shake the furnace, and wait until there is no black smoke coming out of the furnace mouth before adding molten iron.
(2) The operation sequence of filling the furnace bottom is as follows: shake the furnace to the scrap steel adding position, use the scrap steel bucket to load the filling charge into the furnace, the filling charge amount is generally 1~2t; shake the furnace back and forth, generally not less than 3 times, and the rotation angle is at the angle of shaking out the smoke hood at the furnace mouth; open the oxygen to blow the filling charge, generally the gun position is 0.6~1.0m, the oxygen pressure is about 0.6MPa, and the oxygen opening time is about 10s.
(3) Baking. The baking time is required to be 40~60min.
03 Precautions
The precautions for the filling operation process are as follows:
(1) Check the quality of the filling charge to ensure that it meets the requirements.
(2) The amount of filling charge can be less in the early stage of the furnace service, while the amount of filling charge should be more in the middle and late stages of the furnace service.
(3) After the filling is completed, it must be baked for a certain time to ensure the sintering quality.
(4) Since the sintering of the first few furnaces after the filling (especially the first furnace) is not yet sufficient, the furnace should be shaken with special care to minimize the number of furnace reversals. When the furnace needs to be tilted forward or backward, the operator must pay attention to safety and must stand on both sides of the furnace mouth to prevent personal injury caused by sudden collapse of the furnace.
(5) The furnace repair operation must be fully organized and carried out in an orderly manner. Otherwise, it will take too long and the temperature in the furnace will drop too much, which is not conducive to the sintering of the repaired materials.
(6) After the repair, the first and second furnaces must be placed in a conspicuous place on the operating platform in front of the furnace to warn operators to avoid the dangerous area (especially in the direction of the furnace mouth).