Standards for replacing taphole port
(1) The taphole time is less than 3 minutes.
(2) The tapping port is irregular in shape or has obvious pits inside, and the tapping steel is scattered.
(3) The service life of the tapping port is longer than the specified furnace, and it should be arranged in advance according to the production plan.

Methods for replacing taphole port
(1) The plan for replacing tapping port should be issued more than 4 hours in advance to facilitate production organization.
(2) After the steel is tapped and the residue is emptied, the converter is shaken to an appropriate position on the large surface, and the residual steel in the tapping port is cleaned. After the slag splashing of this furnace is completed, the vaporization flue is purged with high-pressure nitrogen to remove the sticky slag.
(3) Shake the converter down to an appropriate position, adjust the tapping port drilling machine to the position to adapt to the tapping port angle, ensure that the drilling angle is accurate, the hole wall is smooth, the hole is round, and the size is appropriate, and avoid damage to the tapping port base brick.
(4) After the tapping port hole is drilled, shake the converter to a position that is convenient for installing the tapping port. While drilling the tap hole, the new tap hole, tap hole material and tap hole material trough should be prepared.
(5) Use a forklift and special tools to place the new tap hole into the drilled channel, adjust the position, and use electric welding to weld the new tap hole guard plate to the tap hole steel plate of the furnace shell for positioning (in order to facilitate positioning, an appropriate amount of tap hole material can be filled into the tap hole before placing the new tap hole).
(6) After the tap hole is positioned, the upper part of the tap hole guard plate should be cut open to facilitate filling of the tap hole material.
(7) Use a forklift and a tap hole material trough to fill the tap hole with an appropriate amount of adjusted tap hole material, fill and compact the end of the gap between the new tap hole and the channel, and ensure that the tap hole is sintered for 3 to 5 minutes. At the same time, adjust the tap hole material after the furnace.
(8) Shake the converter to an appropriate position to facilitate the pouring of material into the taphole, and pour the adjusted taphole material into the gap between the new taphole and the channel. Avoid pouring incompletely during operation.
(9) During the pouring process, timely observation should be made to ensure that there is no leakage. After the pouring is completed, the sintering time should be guaranteed to be more than 15 minutes.
(10) After each taphole change, the slag stopper should be adjusted in time to ensure that the slag stopper cone is accurately positioned.
Requirements for taphole maintenance and replacement
(1) The furnace master should pay attention to the taphole condition for each batch of steel, and confirm the inner and outer mouths of the taphole after the steel is discharged. If the inner mouth is not good, pay attention to the condition of the rear large surface, and do a good job of final slag, and then pour the slag to maintain the rear large surface and the inner mouth of the taphole. If the inner mouth is severely eroded, contact the furnace protection supervisor to come to the site for confirmation in time, take measures, replace the taphole, and maintain the rear large surface.
(2) If the outer mouth of the taphole is severely eroded, it should be repaired in time. If the shaped steel plate is damaged, notify the converter foreman in time. If steel seepage is found at the steel outlet, the furnace supervisor should be notified for on-site confirmation and replacement should be organized in time.
(3) As long as the steel outlet is found to be broken or severely eroded, no matter how many times the steel outlet is used, the furnace supervisor should be notified for on-site confirmation and replacement of the steel outlet should be organized.
(4) If the steel outlet time is less than 3 minutes, the furnace supervisor should be notified for on-site confirmation immediately. The furnace supervisor should report to the dispatch room on-site and coordinate the replacement plan of the steel outlet.
(5) The furnace supervisor should keep abreast of the situation of the steel outlet at any time, determine the time to replace the steel outlet, and report to the planner. When replacing the steel outlet according to the plan, the foreman and the furnace master should arrange to replace the drill bit and clean the furnace outlet.
(6) When drilling the old steel outlet, the second assistant and the furnace master must confirm the correct angle of the drill rod and must not deviate.
(7) Before installing a new taphole, make sure there is no residual steel. If there is residual steel, use a coal oxygen gun to burn it clean to ensure that the inner mouth is uniform and smooth. When installing a new taphole and spraying the outer mouth, the furnace guard must ensure that the taphole is in the correct position before spraying the material. After spraying the outer mouth, use a coal oxygen gun to bake for 3~5 minutes before shaking it to the back of the furnace.
(8) When spraying the back of the furnace, make sure that the material-water ratio is adjusted to the required standard and the viscosity is appropriate before entering the furnace for spraying. Do not adjust the spray gun after it is inserted into the furnace. If a dry self-flowing taphole is used, the temperature must be appropriate and the self-flowing material must have good fluidity so that the inner mouth of the taphole is filled and filled.
(9) Before adding molten iron, make sure that the spraying material is completely dry before adding molten iron.
(10) Before production, make sure that the condition of the taphole is confirmed before adding molten iron. During blowing, if there is flame coming out of the taphole, it means that the taphole is unobstructed.
Measures to extend the life of the steel outlet
(1) Reduce the amount of slag in the early and late stages of steel outlet, and use slag blocking technology to block the slag during steel outlet.
(2) If necessary, the slag can be reversed from the steel outlet after adjusting the slag to reduce the erosion of the steel outlet by the slag.
(3) Reduce the damage to the steel outlet caused by high-temperature steel, over-oxidized steel, etc.
(4) Repair the steel outlet in time to maintain the normal shape and size of the steel outlet.
(5) Use high-quality materials. The material used for the steel outlet is required to be resistant to high temperature, erosion, scouring, and rapid cooling and heating.
Why is the converter taphole considered the weakest and most maintenance-intensive part of the furnace lining?
A: The taphole is subjected to extremely harsh physical and chemical stresses during operation:
High-speed erosion: During tapping, high-temperature molten steel flows at extremely high speeds, generating intense mechanical wear.
Chemical corrosion: Steel slag reacts chemically with the taphole material, leading to material loss.
Hot-cold cycling: The drastic temperature changes between the end of tapping and the next heat cause thermal shock, making the material prone to cracking and spalling.
Oxidation: Under high-temperature conditions, the carbon (from the magnesium-carbon alloy) within the taphole is easily oxidized, weakening the structural strength.
What are the two main methods for replacing the taphole? What are the differences between them?
A: Mainly divided into complete replacement and sleeve replacement (plugging method):
Complete replacement: Applicable when the taphole seat bricks are severely damaged or during major overhauls. It requires removing the old seat bricks and surrounding filler, and reinstalling a completely new taphole composite brick.
Sleeve Replacement: This is a quick maintenance method. When the inner diameter of the taphole expands to the point of affecting tapping time or flow pattern, a thinner refractory sleeve is inserted into the existing taphole hole, and the gap is filled with filler. This method does not require removal of the base bricks, resulting in minimal downtime.
How to determine whether the taphole needs maintenance or replacement through daily observation?
A: On-site operators mainly rely on the following three signals for judgment:
Shortened Tapping Time: If the tapping speed significantly increases (e.g., from 5 minutes to 3 minutes), it indicates that the orifice diameter has been burned and enlarged.
Spreading Flow and Slag Trapping: If the molten steel flow becomes dispersed instead of in a stream, or if slag trapping occurs prematurely, it indicates that the inner wall of the taphole is uneven or its shape has been severely deformed.
Visual Inspection of Residual Thickness: Observe the actual length of the taphole and the condition of the end after furnace operation. If the end is found to be severely red-hot or shortened, immediate action is required.
Why is the operation of “Ramming Material” crucial during taphole replacement?
A: The filler is placed between the taphole sleeve (or seat brick) and the furnace shell/lining. If the filler is not compacted or improperly installed:
Risk of steel seepage: Molten steel may seep into the gaps, even burning through the furnace shell and causing an accident.
Insecure fixation: Insufficient filler strength can cause the taphole to loosen or shift (i.e., “float”) under the impact of molten steel.
Stripping: The quality of the filler directly affects the overall lifespan; high-quality magnesia-carbon ramming mix can significantly extend the service life of the taphole.
What are the precautions for the “baking” stage after taphole replacement?
A: Baking is crucial to ensuring the performance of the new material:
Slow heating: The heating curve must be strictly followed to eliminate volatiles in the filler and binder (such as resin) and prevent instantaneous vaporization of moisture that could cause cracking.
Carbonization bonding: For magnesia-carbon materials, the baking process is a process of resin condensation and carbonization, which determines the final mechanical strength of the taphole.
First heat protection: The first heat of steel produced after replacement usually requires special attention to ensure stable molten steel flow and verify the quality of installation.