During LF refining, submerged arc heating is implemented according to the following power supply and heating regime:

(1) Initial stage – slag crust breaking and arc ignition

Voltage tap T4 and current curve 2 are used to ensure short arc operation and medium voltage, which facilitates arc ignition and slag melting.

(2) Slag melting and temperature rising stage

According to the molten steel temperature, slag forming amount and refining time, voltage taps T4–T8 and current curves 1–3 are selected.

(3) Alloying and final temperature control stage

Higher voltage taps T6–T10 and current curves 1–3 are used so that the target temperature can be reached in a short time.

Except for the initial arc ignition and slag melting stage, submerged arc operation must be maintained throughout the heating process. During heating, the arc sound should remain stable without any abnormal “thunder-like” noise.

The use of high-voltage open arc heating to forcibly adjust temperature is strictly prohibited, as it may damage the ladle refractory lining.

When measuring temperature or taking steel samples, the power must be switched off and the electrodes lifted.

During heating, automatic control should be used preferentially, while manual operation is only used under abnormal conditions.

Under normal circumstances, the heating rate of molten steel is 3–4.5°C per minute.

How to Achieve White Slag Refining in LF Furnace

The slag forming practice of the LF furnace follows the principle of rapid slag melting and early formation of white slag.

After molten steel arrives at the LF station, the slag crust should be broken as quickly as possible.

After the initial slag melts, lime, synthetic slag and premelted slag are added in batches according to the requirements of desulfurization and submerged arc heating.

Bauxite or fluorite is used as a slagging agent to ensure that slag-forming materials melt uniformly within the specified slag formation time.

For steel grades requiring deep desulfurization, additional synthetic slag should be added to increase slag basicity. The final slag basicity should be controlled at R ≥ 3.0. At the same time, the argon flow rate should be appropriately increased and the molten steel temperature raised to ensure sufficient stirring time under a reducing atmosphere.

According to slag conditions and steel grade requirements, small amounts of calcium carbide, ferrosilicon powder or aluminum particles are added to the slag surface in batches through the feeding port to promote the formation of white slag.

The final slag composition must satisfy:

TFe% + MnO ≤ 1%

During the entire process, dual bottom argon blowing is applied. The argon flow rate should be adjusted to meet the metallurgical requirements at each stage.

During argon blowing of fully deoxidized molten steel, the steel surface must not be exposed.

In the middle and later stages of refining, when the sulfur content of molten steel meets the internal control specification, the bottom argon flow rate can be appropriately reduced depending on production conditions.

The pre-argon blowing time should not be less than 3 minutes.

During soft blowing, the argon stirring effect should be such that a “mushroom-shaped” bulging movement appears on the slag surface, but the molten steel surface should not be exposed.

If the bottom stirring effect is insufficient, a pressurizing device can be used to enhance the gas permeability and stirring effect.

Principle of Calcium Treatment

In China, calcium–iron wire is generally powder-filled, which produces large amounts of vapor during wire feeding. The calcium recovery rate is relatively low, and the wire is prone to breakage and jamming, which affects steelmaking operations.

Solid pure calcium wire, on the other hand, consists of a high-density solid calcium core wrapped by a thick steel sheath. The wire has higher rigidity, does not slip or deviate during feeding, and can remain below the critical depth in molten steel for a longer period, significantly improving calcium recovery.

Calcium treatment involves feeding calcium wire into molten steel using a wire feeding machine.

With the assistance of the bottom argon stirring system of the ladle, the molten steel is homogenized. Large high-melting-point brittle Al₂O₃ inclusions produced during deoxidation can be transformed into low-melting-point calcium aluminate inclusions (such as 12CaO·Al₂O₃), thereby promoting the flotation of inclusions and improving the cleanliness of molten steel.

In aluminum-deoxidized steels, alumina inclusions have very high melting points and remain solid at continuous casting temperatures. These inclusions easily accumulate at the tundish nozzle, leading to clogging.

The density of Al₂O₃ inclusions is lower than that of molten steel. If the morphology of aluminum deoxidation products can be controlled so that they exist in liquid form in molten steel, large quantities of these inclusions can be removed before entering the tundish.

This not only reduces tundish nozzle clogging, but also improves steel cleanliness and enhances the quality of continuously cast billets.

Calcium treatment can also prevent the formation of elongated sulfide inclusions, thereby improving the anisotropy of steel.

Therefore, controlling the morphology and composition of MnS inclusions is very important.

Regardless of the aluminum content in steel, after calcium addition, spherical or globular CaS or (Ca,Mn)S inclusions are generally formed, preventing the formation of dendritic MnS inclusions.

Mechanism of Calcium Wire Feeding

Calcium–iron wire is powder-filled, whereas solid calcium wire adopts a thick steel sheath with a solid core.

The core consists of high-density solid calcium rods produced by high-pressure wire drawing. During feeding, it does not introduce additional oxides into molten steel, thus avoiding contamination.

The thick outer steel sheath and high-density calcium core allow calcium to be delivered deeper into molten steel and remain below the critical depth for a longer time, resulting in a higher calcium recovery rate.

In contrast, calcium–iron wire is relatively soft and can only penetrate shallow depths in molten steel.

If the slag layer above molten steel is too thick or becomes agglomerated, the calcium–iron wire cannot penetrate it and may float on the slag layer, causing waste.

As shown in Figure 1, the guide tube of the wire feeder should be positioned slightly away from the bottom argon blowing port.

During wire feeding, the thick-sheathed pure calcium wire follows the vortex generated by argon bubbles and enters deeper regions of molten steel.

After multiple collisions, the solid calcium particles are broken into fine calcium particles, which are uniformly distributed in the deeper molten steel.

This promotes the transformation of inclusions into calcium aluminates and (Ca,Mn)S inclusions.

Since the amount of wire feeding is small, the feeding time is reduced by 2–3 minutes.

When feeding solid pure calcium wire, white smoke emissions are relatively small, making the process more environmentally friendly.

The calcium content in molten steel becomes stable, the fluidity of molten steel improves, and the flotation of inclusions is promoted.

This also contributes to more uniform composition and stable quality of continuously cast billets.

Schematic Diagram of Thick-Sheathed Calcium Wire Treatment
Figure 1 – Schematic Diagram of Thick-Sheathed Calcium Wire Treatment

How to Control the Argon Flow in LF Bottom Blowing

The bottom argon blowing process is a very important part of LF refining.

Its functions include:

  • Stirring molten steel
  • Homogenizing temperature and composition
  • Promoting inclusion flotation
  • Removing non-metallic inclusions and harmful gases

After argon stirring and static holding in the ladle, a short period of argon blowing before continuous casting can further promote the removal of small-diameter inclusions.

During the heating and slag melting stage, the argon flow rate should be controlled at a relatively low level.

This helps to form foamy slag, prevents carbon pickup from electrodes, and reduces heat loss from molten steel.

After slag melting is completed, the argon flow can be adjusted to a medium intensity so that the slag can rapidly undergo deoxidation and form white slag.

Then the argon flow is increased to strong blowing, allowing the highly active white slag to effectively remove inclusions and perform desulfurization.

A certain period of strong stirring should be maintained to ensure effective inclusion removal.

Finally, after calcium treatment, soft argon blowing is applied for a certain period to further remove inclusions.

Influence of LF Refining Slag on Nitrogen Absorption in Molten Steel

The situation is similar to that during electric arc furnace heating. Regardless of whether aluminum deoxidation is applied, the molten steel in areas directly exposed to the arc tends to absorb nitrogen.

Therefore, during LF refining, it is essential to form a good foamy slag layer to prevent exposure of the molten steel surface in the arc zone and to reduce nitrogen uptake in these regions.

Additionally, when the temperature of the refining slag is lower than that of the molten steel (i.e., slag surface temperature between 600–1500°C), nitrogen absorption by the molten steel is minimal. In this case, the refining slag effectively prevents nitrogen absorption.

Maintaining a reasonable slag volume and ensuring that the molten steel remains well-covered by slag throughout refining is crucial for controlling nitrogen uptake.

However, when the refining slag temperature approaches the molten steel temperature, such as during LF heating, nitrogen absorption becomes significant. As temperature increases:

  • The rate constant of nitrogen absorption increases
  • The mass transfer coefficient of nitrogen in slag increases

Therefore, minimizing the time the slag remains at high temperature is beneficial in reducing nitrogen absorption.

When high-power heating is used in combination with foamy slag, molten steel temperature rises rapidly in a short period. The duration of heating is roughly equal to the persistence of the foamy slag. The foamy slag surrounds the arc, which:

  • Improves electrical energy utilization
  • Reduces radiation damage to the refractory lining
  • Shortens the high-temperature duration of the slag

This strategy effectively prevents nitrogen absorption by molten steel.

Effect of Using BaO and CaF₂ in Refining Slag

When the BaO content in refining slag is between 0–10%, the sulfur distribution ratio (Ls) increases rapidly. This is because BaO has stronger basicity than CaO, with an optical basicity approximately 1.15 times that of CaO.

In molten slag, the ionic radius of Ba²⁺ is larger than that of Ca²⁺, resulting in weaker interionic attraction. Moreover, the fraction of ions in BaO molecules is higher than in CaO molecules. As a result, BaO more readily releases oxygen ions (O²⁻). With increasing BaO content, Ls rises quickly.

When the BaO content exceeds 10%, the increase in Ls slows down. This occurs because excessive BaO reduces the total quantity of other basic oxides participating in desulfurization reactions, lowering the effective slag basicity.

When the mass fraction of B₂O₃ in slag is less than 10%, its fluxing effect is comparable to that of CaF₂. Additionally, B₂O₃ causes less environmental pollution, making it a favorable alternative to replace CaF₂ in refining slag.

Measures to Prevent Tundish Nozzle Clogging during LF Process

(1) Calcium Treatment in LF Process

Calcium treatment is one of the most widely used methods to improve the morphology of inclusions in high-aluminum steels.

Because converter slag is strongly oxidizing, a layer of aluminum particles must be added first to deoxidize the molten steel before adding slagging materials. Typically, about 60 kg of aluminum is added, which can be adjusted depending on slag amount. The key objective is to form a glassy slag layer.

Once the glassy slag is formed, Ca-Fe wire is fed into the molten steel to reduce the oxidation of calcium by oxygen in the slag.

As shown in Figure 2, with increasing calcium content in inclusions, Al₂O₃ inclusions transform along the sequence:

Al₂O₃ → CaO·6Al₂O₃ → CaO·2Al₂O₃ → CaO·Al₂O₃ → 12CaO·7Al₂O₃ → 3CaO·Al₂O₃

During this transformation, the melting point of inclusions decreases continuously, eventually forming C12A7 inclusions with a melting point of 1455°C.

The residual calcium content in molten steel significantly influences the effectiveness of inclusion modification. Therefore, during calcium treatment, the aluminum addition must be strictly controlled so that the acid-soluble aluminum content in steel remains between 0.02% and 0.05%, which yields optimal results.

Relationship Between Carbon and Oxygen at BOF Endpoint
Figure 2 – Relationship Between Carbon and Oxygen at BOF Endpoint

(2) Control of Argon Blowing Time during LF Process

In the early stage of LF refining, aluminum particles are added, and strong argon stirring is applied to melt the ladle slag.

However, during the treatment process, soft argon blowing should be used to avoid slag entrainment into molten steel, which can cause reoxidation and inclusion formation.

It can be seen that the optimal soft argon blowing time should be approximately 10 minutes.

Effect of Soft Argon Blowing Time on Inclusion Index
Figure 3- Effect of Soft Argon Blowing Time on Inclusion Index

Currently, MgO-C bricks are the primary refractory material used for ladle linings during secondary refining.

In recent years, due to the need for low-carbon and ultra-low-carbon steel production and extending ladle service life, carbon-free ladle linings have been developed, which significantly improve ladle lifespan.

Furthermore, decarbonization and alkalization of ladle linings are new requirements for clean steel production and represent the future development direction of ladle refractories.

Carbon-free materials include:

  • Monolithic castables (primarily corundum-spinel or corundum-magnesia castables)
  • Precast cast blocks
  • Carbon-free mechanically pressed bricks (Al-Mg or Al-spinel bricks)

Traditional brick linings generally start erosion at brick joints, whereas monolithic castables eliminate this problem, providing excellent thermal shock resistance and longer service life.

However, compared with brick linings, monolithic castables have practical issues, such as:

  • strict requirements for water addition during casting
  • curing temperature control
  • baking procedures

In most steel plants, these conditions are difficult to achieve, causing variations in quality. Additionally, monolithic castables require long preparation times from casting to curing and baking. In older steel plants, these requirements are rarely fully met, and erosion during later stages is rapid, requiring frequent patching and increasing labor intensity. These factors limit the promotion and practical application of monolithic castables.

VOD ladle working lining:

Low-carbon MgO-C bricks have relatively short service life. To prevent carbon pickup in ultra-low-carbon steel, high-alumina fired bricks are used. However, high-alumina bricks have poor thermal shock stability, develop cracks easily, stick to steel, and promote slag adhesion.

The future trend is to use Mg-Ca-C bricks or carbon-free Al-Mg bricks.

  • Mg-Ca-C bricks face challenges such as water resistance and sensitivity to operating conditions, limiting their wider application.
  • Carbon-free Al-Mg bricks, when combined with halide bonding, are beneficial for producing clean steel, especially ultra-low-carbon grades.

Currently, some steel plants use Mg-Cr bricks while still using Mg-C bricks as ladle lining materials.

LF/VD ladle working lining (bottom and molten pool):

MgO-C bricks are used. When slag line bricks are replaced regularly, the ladle can be used for 25–35 heats, showing stable performance. To reduce ladle temperature drop and maintain clean steel, the trend is to use low-carbon MgO-C bricks or carbon-free Al-Mg bricks.

  • VHD and LF/VD slag lines: MgO-C bricks
  • VOD slag lines: Mg-Cr bricks or MgO-C bricks

Slag line MgO-C bricks are severely eroded, often forming a slag groove during ladle service.

Main causes:

(1) Chemical corrosion and mechanical erosion

  • Chemical corrosion is more severe. Oxides in refining slag, such as SiO₂ and CaO, react with MgO in bricks, forming low-melting compounds that are removed by slag.
  • FeO in slag oxidizes carbon in MgO-C bricks, loosening the brick structure.
  • During refining, argon stirring and mechanical interaction between steel and slag further accelerate erosion.

(2) Effect of slag system on MgO-C bricks

  • CaO-Al₂O₃-SiO₂ slag system (lime + bauxite) performs better than CaO-SiO₂-CaF₂ slag system (lime + fluorite).
  • Lime-bauxite slag has higher alkalinity, stronger deoxidation capacity, and maintains viscosity at high temperatures, improving slag foaming and extending slag line life.
  • Fluorite-containing slag at high temperature becomes thin and causes arc reflection, severely eroding the slag line.
  • For S-containing steels, adding silica (SiO₂ ≥ 90%) reduces slag basicity, which is detrimental to basic refractories. Therefore, silica addition should be controlled.

Currently, lime-bauxite slag systems are widely used in LF/VD, effectively doubling slag line lifespan. Decarbonized and alkaline slag line refractories represent the future development trend.

Mg-Cr brick slag line erosion:

  • Mainly caused by chemical mineral reaction at high temperatures and physical-mechanical spalling.
  • Research is needed to develop special Mg-Cr bricks resistant to high-temperature slag penetration and wear.

Factors Affecting Decarbonization of Ladle Slag Line Bricks

To prevent carbon pickup and extend ladle life:

  • Ladle wall and bottom refractories should be decarbonized.
  • Slag line bricks should use low-carbon MgO-C bricks.

Factors to consider for achieving fully decarbonized slag line bricks:

    1. Service life:

Most slag minerals are inorganic nonmetallic materials with properties similar to refractories. High-temperature molten steel is highly fluid, which exacerbates slag penetration and erosion. To extend life of decarbonized bricks, materials must have low wetting with slag and strong resistance to slag penetration. Currently, carbon-free refractories cannot fully resist slag infiltration and erosion, and practical service life is often limited, impacting ladle turnover and plant productivity due to more frequent maintenance.

    1. Cost:

To balance slag resistance, penetration resistance, and service life, high-quality raw materials are required for carbon-free slag line bricks, increasing cost. This is a key limitation for their promotion.

    1. Necessity:

Unless specific steel grades require it, full carbon-free ladle refractories are generally not used, as this can increase production cost.

Principle of Bottom Argon Blowing in Ladle

Bottom argon blowing is carried out through porous bricks, with the primary purpose of producing small, dispersed hydrogen bubbles. This slows the rising velocity of bubbles in molten steel and improves purification efficiency.

The porous bricks are composed of a mixture of high-alumina corundum and mullite with a suitable binder, pressed and sintered at high temperature. The argon blowing pressure is determined according to the height of molten steel.

The principle of bottom argon blowing is as follows: argon at a certain pressure is injected into molten steel through the porous bricks, forming bubbles. Due to buoyancy, the bubbles rise, creating upward flow of molten steel in the gas–liquid region. When bubbles reach the top, the flow turns horizontal toward the ladle wall, then flows downward near the wall and returns to the lower part of the ladle, forming a circulating flow (Figure 4).

Argon stirring promotes chemical reactions between steel and slag. During circulation, large inclusions and deoxidation products are transferred into the top slag through the lower part of the top slag region, accelerating material transfer between steel and slag and facilitating deoxidation and desulfurization.

Argon bubbles also create a relative vacuum in molten steel, helping to capture and remove dissolved gases. Moreover, argon stirring ensures uniform composition and temperature in molten steel.

Principle of Ladle Bottom Argon Blowing
Figure 4 – Principle of Ladle Bottom Argon Blowing

Relationship Between Argon Flow Rate and Inclusion Removal

During argon refining, when the gas flow rate is low, small bubbles adhere to and remove inclusions efficiently.

Within a moderate flow range, inclusion removal efficiency does not vary significantly. Relatively larger gas flow increases turbulence in the ladle, promoting collisions and growth of inclusions, which aids in removing more inclusions, resulting in better overall removal.

However, as gas flow continues to increase, inclusion removal efficiency may decrease. This is because bubble diameter increases with flow rate, while bubble number decreases, which reduces adhesion efficiency for inclusion removal.

Further increase in gas flow allows large bubbles to remove inclusions primarily through bubble wake entrainment (Figure 5). With increasing gas flow, bubble diameter and rising velocity increase, which enhances inclusion entrainment.

Once gas flow reaches a certain level, bubble diameter and velocity stabilize, and further increasing flow has little effect on inclusion removal.

The main advantage of large gas flow is that increased turbulence enhances collisions of inclusions, and small inclusions are more easily entrained in the wake of large bubbles rather than being removed by adhesion. Excessive gas flow, however, can cause slag entrainment at the steel surface, contaminating molten steel. Therefore, argon flow should be optimized, balancing inclusion removal and slag surface stability.

Inclusion Removal by Bubble Wake Flow
Figure 5 – Inclusion Removal by Bubble Wake Flow

Mechanism of Chemical Oxidation Erosion of MgO-C Bricks in Ladle Slag Line

During refining, the ladle slag line operates under high temperature, vacuum, and strong stirring, resulting in severe erosion. Slag grooves or even cavities frequently appear, severely reducing service life.

MgO-C bricks at the slag line are initially damaged at brick joints. Intense mechanical action from steel and slag causes broken or spalled brick surfaces to be smoothed, forming a convex “bun-shaped” erosion pattern. Over time, slag penetrates joints and cracks, sometimes causing steel leakage, which accelerates slag line brick failure and shortens working layer service life.

Erosion by slag oxides occurs in two ways:

  1. Melting of MgO grains by slag oxides such as SiO₂ and CaO, forming low-melting compounds that are carried away by slag.
  2. Oxidation of carbon in MgO-C bricks by FeO in slag. FeO reacts with C to form CO, which then reacts with MgO to form low-melting (Mg,Fe)O solid solutions that are easily eroded by slag, loosening brick structure.

High temperature and vacuum exacerbate chemical erosion. At atmospheric pressure below 1600°C, carbon loss is minimal; at vacuum (~1300°C), carbon loss accelerates; above 1600°C, carbon loss increases sharply. As C content decreases, MgO grains are more susceptible to corrosion and oxidation by steel slag.

Mechanism of Mechanical Erosion of MgO-C Bricks in Ladle Slag Line

In addition to chemical erosion, slag line MgO-C bricks are subject to thermo-mechanical wear and abrasion.

  • Thermo-mechanical erosion (spalling) arises from thermal expansion or mechanical vibration-induced stress. Alkaline MgO-C bricks are particularly sensitive due to the high thermal expansion coefficient of MgO.
  • Heating induces volumetric changes; rapid heating can generate excessive thermal expansion, degrading internal brick structure. Stress concentrates at brick ends, crushing corners and edges.

During tapping, high-temperature steel accelerates turbulent mixing with slag, increasing temperature gradients in bricks and generating internal cracks.

LF refining under high temperature and reducing atmosphere combined with low-viscosity molten slag increases mechanical erosion at the slag line. Vacuum argon stirring further aggravates erosion, causing severe wear and reduced service life.

Technical Measures to Extend Slag Line Service Life

    1. Stabilize refining slag composition

    • Slag basicity and composition strongly affect slag line service life. Increased CaF₂ content significantly reduces life.
    • Using a CaO-SiO₂-Al₂O₃ ternary slag system with basicity 3.5–5.0 ensures strong deoxidation, moderate viscosity, and high-temperature adaptability.
    • Good foaming of slag during refining stabilizes the arc, reduces thermal radiation and chemical corrosion, and improves slag line longevity.

    1. Improve ladle construction methods

    • Dry masonry is used at the slag line to reduce thermal expansion damage.
    • MgO-C bricks are installed at the working layer, with high-alumina castable filling along the ladle wall.
    • A thick hardboard is inserted between every three bricks to provide expansion allowance. During baking, the board burns out leaving small gaps; brick expansion compensates the gaps, reducing stress concentration at ends.

    1. Proper ladle baking

    • Maintain and stabilize gas pressure to ensure effective baking.
    • Baking temperature >900°C. Ladles should be used immediately after baking to prevent oxidation or decarbonization of bricks.
    • If ladle cannot be used immediately, low-temperature baking or deferred baking may be applied.
    • Minimize temperature differences between ladle and molten steel to reduce internal thermal stress and prevent cracking or spalling.

Operation of Full-Process Bottom Argon Blowing

Full-process bottom argon blowing begins immediately when molten steel leaves the furnace, continuing until the ladle reaches the continuous casting facility (Figure 6).

  • Argon is supplied via steel pipes to the hose reel, with valves and pressure gauges for control.
  • A rotating joint feeds argon into the hose, which follows the ladle car automatically.
  • Quick couplings are used to connect hoses to the ladle for convenience and safety.

Operation sequence:

  1. Place empty ladle on ladle car → connect hose via quick coupling
  2. 30s after tapping, open argon valve, maintaining 0.15–0.2 MPa
  3. Add scrap and feed wire for temperature control
  4. Ladle car moves to endpoint → close argon valve, disconnect quick coupling → LF refining → continuous casting

Full-process argon blowing:

  • Requires no additional operating area or time
  • Equipment is simple, low investment, quick effect
  • More uniform temperature and composition than top-blowing plugs

Injected argon forms countless small bubbles, which expand in hot steel, producing circulation 50–100 times the argon volume, creating strong stirring.

  • Excessive argon flow may cause steel splashing, surface turbulence, and secondary oxidation.
  • Optimal argon intensity is critical.
Full-Process Ladle Bottom Argon Blowing System
Figure 6 – Full-Process Ladle Bottom Argon Blowing System

Characteristics of Regenerative Ladle Baking Devices

During transport and pouring, ladle loses significant heat, mainly from refractory lining (~45–50% of total heat loss).

Therefore, preheating is essential.

Regenerative ladle baking system (Figure 7) consists of:

  • regenerator chamber, ladle cover, blower, induced draft fan, reversing valve, and control valves

Working principle:

  • Burners preheat air, with honeycomb ceramic regenerators storing heat.
  • Waste gas heats fuel gas and combustion air.
  • Reversing burners alternately combust, with one burning while the other regenerates and vents.
  • Air temperature exceeds 1000°C, accelerating ladle heating and improving energy efficiency.

Advantages:

  • Faster and more uniform heating
  • Reduced fuel consumption
  • Shorter ladle turnaround
  • Lower refractory consumption
Regenerative Ladle Baking Burner System
Figure 7 – Regenerative Ladle Baking Burner System

Disadvantages of Using Quartz or Ordinary Al-C Submerged Nozzles for Ultra-Low-Carbon and Clean Steel Casting

Quartz nozzles inherently have poor thermal stability, which often leads to nozzle cracking or rupture during pouring, as well as poor resistance to erosion. This also increases the risk of silicon pickup in continuous casting.

Although ordinary aluminum-carbon (Al-C) nozzles have better resistance to erosion, when casting ultra-low-carbon steel, they can cause carbon pickup in the molten steel.

Heat Transfer Mechanism of Molten Steel Loss in Ladle

The heat loss mechanism of molten steel in the ladle is shown in Figure 8.

  1. Molten steel in direct contact with the ladle wall transfers heat to the wall via conduction. Part of the heat is stored in the wall, and part is dissipated to the surrounding environment via radiation and convection.
  2. Heat is also lost through the steel surface by conduction, radiation, and convection.

Regardless of slag thickness, convection occurs inside molten steel, affecting the pouring temperature differently:

  • Thin slag layer: Temperature loss at the steel–slag interface exceeds internal temperature differences. Surface steel becomes denser and sinks, mixing with central steel, preventing temperature stratification.
  • Thick slag layer: Thick slag provides insulation. Heat loss at the steel–slag interface is minimal (though not zero). Conduction through the side walls lowers adjacent steel temperature, forming sidewall steel convection. This flow reaches the ladle bottom, causing temperature stratification, directly influencing pouring temperature.

Changing the material or thickness of the insulation layer is the most effective way to reduce heat loss and surface temperature of the ladle. Reducing insulation thermal conductivity is particularly effective. Modifying working or permanent layer thickness has less impact unless thermal conductivity is changed.

Without insulation, ladle wall and bottom surface temperatures can differ by nearly 40°C, significantly affecting steel temperature drop.

Heat Transfer Mechanism in Steel Ladle
Figure 8 – Heat Transfer Mechanism in Steel Ladle

Effect of Water Leakage from Water-Cooled Ladle Covers on Cast Product Quality

Water-cooled ladle covers include three lifting ears and hydraulic cylinders, insulated via flanges to prevent induced currents.

During operation, the cover lowers onto the ladle, leaving a ~100 mm gap above the ladle rim, forming an inert gas atmosphere beneath through argon bottom blowing (Figure 9).

The cover contains 13 water-cooling rings, each with 15 m³/h cooling water.

If water leaks into the molten steel, H⁺ and OH⁻ ions are introduced. During casting, H⁺ is reduced to H₂, which reacts with carbides (CH₄ formation), creating gas porosity in the billet. This causes internal defects and reduces mechanical properties, especially critical for heavy rail steel.

Thus, water leakage directly impacts molten steel quality and billet integrity.

Water-Cooled Ladle Cover Structure
Figure 9 – Water-Cooled Ladle Cover Structure

Judging Slag Properties by Color and Morphology

LF furnace slag color changes with oxidation state, and slag basicity affects physical state. Observing slag appearance can indicate oxidation and basicity.

In practice, use an oxy-gas tube to attach slag samples from the ladle for observation:

  1. Black: Strongly oxidizing, [w(FeO)+w(MnO)] > 2%, lacks reducing ability.
  2. Gray to brown: Moderately oxidizing, [w(FeO)+w(MnO)] = 1–2%, some desulfurization capacity; may require further reduction using C powder or SiC.
  3. White to yellow: Strongly reducing, [w(FeO)+w(MnO)] < 1%, effective for desulfurization. Yellow indicates desulfurization has occurred; increasing slag quantity enhances desulfurization.
  4. Green: Presence of Cr₂O₃, for Cr-containing steel.
  5. Thick smooth pieces (2–4 mm): Good basicity, maintains flowability, promotes desulfurization.
  6. Glassy flakes: High SiO₂, Al₂O₃, or CaF₂ content; low basicity. Add lime to increase slag basicity.
  7. Rough, uneven slag: High basicity, un-melted lime present; adjust by adding Al₂O₃ synthetic slag or fluorite.

Measures to Improve LF Desulfurization Efficiency

Before tapping, an appropriate amount of top slag is added to the ladle. The impact energy of steel flow and steel sensible heat melts the top slag, facilitating early slag formation and reducing total slag required in LF.

To ensure lime fully melts, use a 4:1 mixture of lime to fluorite as refining slag. Weighting and feeding devices add this top slag evenly before tapping. The top slag modifies and pre-deoxidizes ladle slag, increasing slag basicity and reducing oxidation, providing early slag formation, pre-deoxidation, and pre-desulfurization effects.

Using high-grade SiC powder for reducing slag:

  1. SiC quickly removes oxygen from slag, forming reducing slag, and SiO₂ reacts with top slag to promote slag formation.
  2. C–O reaction generates bubbles, improving flow and foaming of slag, increasing steel–slag contact area, enhancing desulfurization, and improving inclusion adsorption while reducing steel gas content.
  3. Timely addition of SiC maintains reducing atmosphere, preventing FeO increase in slag.
  4. Foaming with SiC is more stable than conventional foaming agents, improving arc coverage and electrode heating, and preventing carbon pickup in molten steel.

Corrosive Factors Affecting Refining Ladle Refractories

Recent intensification of refining, increased continuous casting and secondary refining ratios, higher tapping temperatures, longer steel residence, and more argon and vacuum operations have imposed harsh conditions on ladle refractory linings:

  1. High temperature: Arc reheating raises slag line temperatures. Slag flow and erosion increase with temperature; unstable arcs may produce hot spots.
  2. Corrosive slag: LF refining uses synthetic slag containing fluorite, lime, and carbide, with highly corrosive calcium aluminate and calcium fluoride.
  3. Long holding time: Up to 4–5 h, increasing refractory erosion and steel penetration.
  4. Intense stirring: Continuous argon bubbling increases mechanical wear of lining.
  5. Vacuum: Accelerates reactions between refractory bricks and steel, degrading lining structure.
  6. Intermittent ladle operation: Large temperature fluctuations (1650°C when tapping, <900°C when empty), with rapid heating/cooling, exacerbate stress and spalling.

MgO‑C bricks have excellent slag corrosion resistance, thermal shock resistance and high‑temperature strength, adapting to severe erosion environment at slag line.

The main trends of ladle refractories are carbon‑free, alkaline and long service life, such as carbon‑free Al₂O₃‑MgO unburned bricks and corundum‑spinel castables.

Adopt effective calcium treatment, control acid‑soluble aluminum content, optimize soft blowing time and use high‑performance refining slag to modify inclusions.

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information