With the implementation of the steel production restriction policy, the shortage of molten iron has become more serious, and the amount of scrap steel has increased year by year. At the same time, with the large-scale consumption of high-grade iron ore resources and high-quality coking coal resources at home and abroad and the increasing pressure of energy conservation and emission reduction, the production cost of blast furnace molten iron is gradually increasing. Therefore, how to maximize the steel production without increasing the iron production has become the primary consideration of the steelmaking system. Considering the factors such as converter loading, smelting heat balance, converter lining maintenance, product quality and comprehensive cost, a high scrap ratio smelting plan is planned to reduce production costs and increase economic benefits.
1 Impact of high scrap steel ratio on converter smelting process
1.1 Impact of high scrap ratio on converter loading
High scrap ratio means the maximum consumption of scrap steel. The converter basically uses scrap steel troughs to add scrap steel. First, different types of scrap steel are loaded into the scrap steel trough by matching, and the scrap steel trough is hoisted by the charging cross crane to add the scrap steel into the converter. With the continuous increase of scrap ratio, the scrap steel trough of some enterprises cannot meet the single bucket loading, and the scrap steel trough is expanded, heightened and lengthened. Although the amount of scrap steel added has increased, the total tonnage of scrap steel + trough exceeds the design tonnage of the charging cross crane, which does not meet the regulatory requirements. Considering the high investment cost of the crane transformation, the crane has not been transformed, which limits the improvement space of the scrap steel ratio; another part of the enterprises choose to add scrap steel with double buckets. Although this mode solves the problem of crane overload, it increases the converter smelting cycle and seriously affects the converter production efficiency. Therefore, in order to fundamentally solve the problem of scrap steel entering the furnace under the high scrap steel mode, other ways of adding scrap steel other than directly feeding scrap steel into the converter need to be considered.
1.2 Impact of high scrap ratio on steel consumption index
Scrap ratio is a key factor affecting steel consumption index. Through the high scrap ratio smelting practice of Yulin Steel’s 120t top and bottom double-blown converter, the recovery rate of different types of scrap steel is different. According to the proportion of scrap steel purchased by Yulin Steel, the scrap recovery rate is about 87.27%. According to the composition of Yulin Steel’s molten iron and the total slag of the converter, the molten iron recovery rate is about 91.85%. Because the molten iron recovery rate is greater than scrap steel, the steel consumption index increases by about 0.0458kg/t for every 1kg/t increase in scrap steel consumption.
1.3 The influence of high scrap ratio on converter smelting process
(1) The melting of scrap in the converter pool needs to go through three processes: surface molten iron condensation, condensation layer melting, and scrap carburization melting. According to the 120t top and bottom double-blowing converter smelting practice of Yulin Steel, under the high scrap ratio mode, the scrap entering the converter is not less than 32t. In the early stage of blowing, small and medium-sized scrap and plate-shaped scrap with large surface area melt quickly. The temperature of the converter pool drops significantly in the early stage of blowing. The dust removal system of the Yulin Steel converter is dry dust removal. In order to control the explosion during the opening of the blow, the dry dust removal adopts low oxygen pressure ignition. The phenomenon that the converter lower gun fails to ignite within 50s of oxygen supply is quite frequent. (2) When molten iron is added to the converter, some scrap steel is melted. In the early stage of blowing, the temperature of the molten pool is low, the heat and mass transfer of the molten pool is slow, and the temperature of the molten pool rises slowly. In addition, other scrap steel melts quickly, which slows down the heating rate of the converter. It is difficult to slag after the first batch of auxiliary materials are added to the converter, and the dephosphorization efficiency of the converter decreases in the early stage of blowing. Yulin Steel adopts a one-pot system for loading molten iron. Affected by the turnover rate of the molten iron tank, the temperature of the molten iron in a single tank varies greatly. In the early stage of smelting, it is necessary to flexibly adjust the amount and timing of auxiliary materials according to the process temperature. The temperature control during the smelting process is difficult. Low-temperature slag overflow and unstable dephosphorization rate are prone to occur in the early stage of smelting. Poor slag formation in the middle stage is prone to dryness, resulting in a lower end carbon temperature hit rate and an increase in the number of overoxidation furnaces.
1.4 Impact of high scrap ratio on converter lining
According to the practice of 120t top and bottom double-blown converter smelting in Yulin Steel, in order to increase the scrap ratio, the scrap material type is mainly heavy scrap steel above 6mm. During the process of scrap steel entering the furnace, the impact on the large lining of the front of the converter is large, causing certain damage to the large lining of the front of the converter. During the smelting process, the oxides and non-metallic impurities in the scrap steel have a certain erosion effect on the refractory materials of the converter. At the same time, the temperature of the molten pool is low in the early stage of smelting, slagging is difficult, the slag basicity is low, and the lining is seriously eroded. Due to the low calorific value of scrap steel, high scrap ratio loading cannot provide enough heat, the converter process temperature is not surplus, and the terminal temperature of some furnaces is insufficient, which does not meet the converter tapping temperature standard. It is necessary to blow out the steel. The carbon content at the end of the spot blowing furnace is low, the molten steel is highly oxidizable, the FeO content in the slag is high, the converter splashing slag protection effect is poor, and the difficulty of converter furnace condition maintenance increases.
1.5 The influence of high scrap ratio on molten steel quality
The scrap steel entering the converter is mainly purchased scrap steel, which is of mixed materials and difficult to distinguish. The trace elements such as sulfur, chromium, and copper in the scrap steel are unstable. The high scrap ratio smelting increases the amount of sulfur returned in the converter. At the same time, the nitrogen content of the molten steel terminal tends to increase. The sulfur and chromium content at the converter terminal are often high, which affects the quality of the steel billet and the rolling performance of the steel.
2 Analysis of control measures for the impact of high scrap steel on steelmaking process
2.1 Control measures for high scrap ratio scrap steel feeding into the furnace
According to the production practice of 120t top and bottom combined blowing converter in Yulin Steel, in order to maximize the scrap ratio, process adjustments and improvements are mainly made from the following aspects.
(1) Optimization of scrap steel material type. In order to ensure the loading of scrap steel in a single bucket and maximize the scrap ratio, it is crucial to increase the purchase proportion of heavy scrap steel or reduce the size of scrap steel to increase the pile density. The purchase size of the purchased scrap steel used in the 120t converter is recommended to be controlled within 1000mm×600mm, and the pile density reaches more than 1.15t/m3, which can meet the requirements of single bucket loading of scrap steel.
(2) Adding scrap steel to the blast furnace hot metal tank. The thermal balance of the converter depends on the difference between the heat income and heat expenditure of the charge. Making full use of the physical heat and chemical heat of the molten iron to optimize the structure of the metal material entering the furnace is an important way to improve the scrap ratio. Yulin Steel adopts a molten iron one-pot smelting process. The turnover rate of the molten iron pot is about 2h/time. The blast furnace tapping temperature is 1510℃~1540℃, and the converter molten iron temperature is 1350℃~1450℃. The molten iron has excess heat. Before the molten iron pot is assigned to the blast furnace, 5t~6t of scrap steel is added to the molten iron pot. The heat and impact force during tapping are used to melt part of the scrap steel in the molten iron pot and directly convert it into liquid iron, thereby reducing the converter molten iron temperature, making the converter smelting process optimal, effectively improving the scrap ratio, further reducing iron consumption and increasing steelmaking capacity.
(3) Adding scrap steel to the ladle after the furnace. Purchase some steel bar cut heads or use pure scrap steel produced by rolling mills. The length is controlled within 10cm. After this part of the scrap steel is baked in the post-furnace baking furnace, it is added to the ladle along with the steel flow during the converter tapping process. The amount added to a single furnace is controlled at about 1t, and the temperature loss of the molten steel is about 10℃, which can maximize the scrap ratio.
2.2 Control measures for steel consumption index under high scrap ratio mode
The scrap steel recovery rate is lower than the molten iron recovery rate. The high scrap ratio will inevitably affect the increase of steel consumption index. Under the high scrap ratio mode, the converter end point FeO can be reduced to less than 12% by measures such as less slag retention in the converter and the end point gun pressure time of not less than 90s. At the same time, the appropriate amount of auxiliary iron-containing materials such as dust removal ash balls and sludge balls can not only help the process slagging and prevent the loss of return drying and splashing, but also recover a certain proportion of metal to reduce the steel consumption index, so that the steel consumption index is controlled at a reasonable level.
2.3 Control measures for high scrap ratio smelting process
(1) Optimize the converter slag making process. According to the practice of high scrap ratio smelting in 120t top and bottom combined blown converter of Yulin Steel, the converter process temperature of high scrap ratio smelting mode is not surplus, the smelting process adopts less slag retention process, and only active lime and magnesium balls are used as auxiliary materials for slag making. The consumption of magnesium balls is controlled at 6kg/t~8kg/t. After the slag splashing of each furnace of steel is completed, 25%~100% of slag is retained in the furnace according to the final slag conditions for the next furnace of steel smelting. It can not only alleviate the problem of low slag slagging in the early stage of converter smelting, but also make full use of calcium oxide in the slag of the slag furnace to reduce the consumption of active lime. The characteristics of the high scrap ratio smelting mode are low temperature and difficulty in slagging in the early stage. The use of iron slag formation path is conducive to scrap steel melting and rapid slagging. In the actual smelting process, slag-forming agents need to be added in batches. The first batch is mainly magnesium materials, and the addition time is delayed by 1min to 2min, which is conducive to the melting of scrap steel and the rapid heating in the early stage. In the early stage, the MgO content is increased to protect the splashing slag layer, and the FeO content is increased to promote slagging. Later, according to the slagging situation, slag materials are added in batches to gradually increase the CaO content in the slag.
(2) Optimization of the first batch of auxiliary materials and oxygen supply system. The amount of scrap steel entering the converter increases. In order to ensure the temperature balance and good slagging during the smelting process, the first batch of auxiliary materials and oxygen supply intensity are adjusted as follows. Control of the first batch of auxiliary materials. While ensuring that the total amount remains unchanged, add them in batches. It is strictly forbidden to add the first batch of auxiliary materials to the furnace at one time; the subsequent auxiliary materials are added according to the principle of adding multiple batches in small quantities, and the amount of each batch is controlled at 500kg to 800kg. Gun position control. During the ignition of the lower gun, the gun position height is controlled according to 800mm of the measured liquid level; after the fire is ignited and the first auxiliary material is added, the oxygen gun position is controlled according to 100mm of the measured liquid level; during the smelting period from the start of the carbon-oxygen reaction to carbon pulling, the oxygen gun position is controlled according to 200mm~300mm of the measured liquid level; during the final carbon pulling, the oxygen gun position is controlled according to the measured gun position. In terms of oxygen flow control. Combined with the characteristics of dry dust removal, the oxygen flow during ignition is adjusted according to 18000Nm3/h~22000Nm3/h to prevent explosion during ignition. The oxygen flow of the fire is adjusted to 30000Nm3/h. Increasing the oxygen flow increases the impact depth and strengthens the stirring, which is conducive to rapid heating in the early stage to ensure the first batch of auxiliary materials are thoroughly melted. After the carbon-oxygen reaction begins, the oxygen flow rate is adjusted to 28000Nm3/h~28500Nm3/h. The oxygen flow rate is reduced to slow down the carbon-oxygen reaction rate, so that the molten pool is heated evenly, the FeO content in the slag is guaranteed, and the drying phenomenon is alleviated. After 12 minutes of oxygen supply for smelting, the oxygen flow rate is adjusted to 30000Nm3/h to strengthen the stirring of the molten pool, uniform composition and temperature, stabilize the flame, facilitate carbon pulling, reduce the FeO content in the slag, and improve the metal recovery rate.
(3) After the scrap ratio is increased, in order to improve the hit rate of the converter terminal carbon temperature, the first is to reduce the tapping temperature. Through measures such as tapping port expansion, ladle cover, alloy scrap steel post-furnace baking, and ladle nano insulation, the tapping temperature is reduced by 15℃. The second is to establish a smelting model under different scrap ratio modes. According to the temperature of the molten iron entering the furnace, the timing of auxiliary material addition and the oxygen lance blowing position are reasonably selected to ensure the slag-removing effect and the control accuracy of the slag system components during the smelting process, which is more conducive to the control of the converter smelting process.
2.4 Control measures for high scrap ratio converter lining
According to the high scrap ratio smelting practice of Yulin Steel’s 120t top and bottom combined blowing converter, under the high scrap ratio mode, the first is to adopt slag-retaining and less slag operation, the slag-retaining furnace blows the early slag block, and the slag is quickly slaged after adding magnesium materials in the early stage. The slag has high MgO and CaO content, which inhibits the erosion of the early furnace lining. Second, magnesium balls with high MgO content are used to replace light-burned dolomite, reducing the total slag volume of the converter by about 8kg/t, reducing the temperature loss caused by the large amount of auxiliary materials added during the converter smelting process, and reducing the converter tapping temperature by about 15℃ through measures such as expanding the tapping port, covering the ladle, and preheating the alloy and scrap steel baking furnace behind the furnace, reducing the thermal erosion of the furnace lining; third, pig iron blocks, rolled steel cutting heads and steel bar cutting heads are used to fill the large slag in front of the converter, 3 to 4 times a day for a single furnace, reducing the impact of the converter adding scrap steel on the furnace lining; fourth, the low basicity and low MgO furnace protection process is studied, and the auxiliary material structure is continuously optimized. The basicity of the converter final slag is controlled at 2.3 to 2.5 times, and the final slag MgO is controlled at 5% to 7%. On the basis of ensuring the stability of the converter liquid level, the slag FeO is controlled not to exceed 12%, the furnace condition is stable, and the converter furnace life can reach more than 20,000 furnaces under the converter direct continuous casting machine organization mode.
2.5 Quality control measures for molten steel with high scrap ratio
Strictly controlling the quality of scrap steel is one of the key measures in the high scrap ratio smelting process. The chemical composition of scrap steel is very important for controlling the smelting reaction. In the smelting process with high scrap ratio, adding appropriate amounts of protective agents and alloying elements is very important for controlling the smelting reaction and improving product quality. Scrap steel may contain some oxides, impurities and other harmful components, which will have an adverse effect on the quality of steel during the smelting process. In order to reduce the impact of these substances on the smelting process, operators need to add appropriate protective agents such as silicon, aluminum, calcium, etc. These protective agents can react with harmful components such as oxides to form stable compounds or inclusions, thereby reducing their impact on steel. In addition, according to the requirements of the product and the required composition and properties of the steel, some alloying elements may need to be added. These alloying elements can alloy with other elements in the steel during the smelting process to adjust the composition and properties of the steel. For example, adding manganese can improve the strength and toughness of steel, adding chromium can increase corrosion resistance, and adding nickel can improve plasticity and low temperature resistance, etc. By adding the right amount of protective agents and alloying elements, the smelting reaction can be effectively controlled and the quality of the product can be improved. This requires the operator to make reasonable selection and control according to the specific scrap steel composition and process requirements. At the same time, close furnace condition monitoring and real-time adjustment are also the key to ensure the stability of the smelting process and the consistency of product quality.
Through chemical analysis methods, such as spectral analysis or chemical analysis, the main element content of scrap steel, including iron, carbon, silicon, manganese, etc., can be determined. These data can be used to adjust the steelmaking process to ensure a suitable smelting reaction. There may be impurities in scrap steel that are not conducive to smelting and product quality. For example, excessive sulfur content may lead to the formation of sulfides during smelting and affect the quality of steel.
Therefore, impurity detection such as sulfur content, oxide content and non-metallic inclusions is required. The particle size distribution of scrap steel has an impact on the melting and reaction rate during steelmaking. The particle size of scrap steel can be tested by screening or laser particle size analysis to ensure that it is within a reasonable range to facilitate uniform melting and smelting reactions in the furnace. In addition to testing the quality of scrap steel, appropriate screening measures should be taken, such as selecting reliable scrap steel suppliers and ensuring that their quality control systems are sound, to obtain high-quality scrap steel raw materials. Scrap steel is classified according to its type and characteristics to better control its use in the smelting process. Different types of scrap steel may have different effects on the smelting process, so they need to be classified and processed according to needs. By strictly controlling the quality of scrap steel and taking necessary testing and screening measures, it can be ensured that the scrap steel meets the requirements and minimizes its impact on the steelmaking process. This will help maintain the stability of the smelting process and the consistency of product quality.
3Results achieved
Through the optimization and improvement of the above process, Yugang’s 120t top-to-bottom combined blowing converter for steelmaking has achieved a scrap ratio of more than 26% without adding heat-generating agents such as coke powder and ferrosilicon and without scrap preheating, and the converter smelting indicators have been effectively improved. , after process optimization, scrap steel consumption increased by 55kg/t, and indicators such as the converter end-point carbon temperature hit rate, end-point phosphorus content, final slag FeO, and abnormal composition heats were significantly improved, and the end-point sulfur return and nitrogen increase were effectively controlled. In the continuous caster mode, the converter conditions are stable and the converter age exceeds 20,000 furnaces.
4 Conclusion
By summarizing and analyzing the smelting process problems of low iron consumption and high scrap ratio in Yugang Steelmaking, we formulated control measures and optimized the converter steelmaking process. The specific conclusions are as follows.
(1) In view of the difficulty in adding scrap steel to the converter under the high scrap ratio mode, the first is to optimize the size of the scrap steel material, the size of the purchased scrap steel should not exceed 1000mm×600mm, and the pile specific gravity should not be less than 1.15t/m3; the second is to tap the iron in the hot metal tank Before adding a part of small and medium-sized scrap steel to the molten iron tank, the iron flow from the blast furnace is used to stir and melt. The impact on the temperature of the molten iron entering the furnace is controlled. According to the steelmaking production practice of Yugang Steel, a single tank is equipped with 6 tons of scrap steel. The temperature loss of the molten iron before entering the furnace is 20 ℃ ~ 30 ℃, the hot metal tank capping or the hot metal tank scrap steel preheating technology can be used to reduce the process temperature loss and further improve the scrap ratio; thirdly, 1t of baked steel bar cut ends are added to the post-furnace tapping process, and the temperature loss is about Around 10℃, it can be selectively added according to the end temperature of the converter, which fundamentally solves the problem of loading the converter when the scrap ratio is high. (2) Under the high scrap ratio mode, the converter adopts the slag-less and slag-retaining mode, which is beneficial to the converter process operation and index improvement. According to the end point control situation, after the slag splashing is completed, 25% to 100% of the slag is left in the furnace for use in the lower furnace. On the one hand, it can promote rapid slag removal in the early stage of converter smelting. The high CaO and MgO content of the early stage slag not only inhibits the impact of acidic slag on the furnace in the early stage The erosion of the conditions, and the phosphorus removal effect is obvious, the FeO content of the final slag is reduced by about 2%; on the other hand, through the operation of reducing slag and leaving slag, the consumption of active lime and magnesium balls is minimized, and the consumption of lime is reduced by about 5kg/t, and the consumption of magnesium is reduced by about 5kg/t. The ball consumption is reduced by about 3kg/t. On the premise of ensuring the stability of the smelting process, it effectively reduces the cost of converter smelting auxiliary materials and is more economical. (3) In the high scrap-to-steel ratio smelting mode, the converter only uses active lime and magnesium balls to make slag. The alkalinity of the final slag is controlled at 2.3 to 2.5 times, and the MgO of the final slag is controlled at 5% to 7%. Yugang Steelmaking 120t Top The liquid level of the bottom double-blown converter is controlled to be no less than 1.8m, the converter operates stably, and the furnace age can exceed 20,000 furnaces.