Titanium ore or titanium balls are a common method for blast furnace operators to protect blast furnaces. However, when the titanium content of hot metal increases to 0.12%-0.28%, it has many adverse effects on the operation of the steelmaking process, mainly reflected in: the consumption of slag and steel materials in the converter smelting process increases, and the effect of slag splashing and furnace protection becomes worse. Therefore, research on the smelting technology of titanium-containing hot metal is of great significance to reducing smelting costs and reducing or eliminating the impact of increased titanium content in hot metal on steelmaking operations.
The influence of high-titanium hot metal on converter operation

1. During the converter smelting process, titanium is oxidized before silicon, forming titanium oxide (TiO2) into the slag, which reduces the melting point of the slag and increases the viscosity; it makes the slag difficult to penetrate, resulting in the inability to fully separate the steel-slag at the converter end, and increasing the consumption of steel materials.
2. TiO2 is easy to combine with CaO, resulting in a decrease in the utilization rate of white ash and an increase in the frequency of excessive phosphorus and sulfur at the end of smelting.
3. It causes an increase in the number of re-blowing furnaces, overoxidation of molten steel, and a high FeO content in the converter slag, which worsens the effect of splashing slag to protect the furnace.
4. In addition, the sticky slag adheres to the inside of the furnace mouth, causing the furnace mouth to become smaller and the scrap steel to be difficult to enter the furnace, which has brought many adverse effects on production.
Optimization plan for smelting high-titanium molten iron
For high-titanium hot metal, the main problems to be solved are slag stickiness, poor slag formation during the process, poor dephosphorization effect, and non-separation of steel and slag at the end. The optimization plan is as follows:
1. In the early stage of smelting, high gun position operation is adopted, and FeO materials are added at the same time. The high gun position operation in the early stage increases the FeO content in the slag, accelerates the melting of lime, and adds a large amount of lump ore at the same time to maintain a high FeO content in the slag, that is, it is controlled according to the iron slag formation pathway, which can increase the fluidity of the slag and facilitate the pouring of the high TiO2 viscous slag.
2. The key to the operation in the middle and late stages is slag formation. It is necessary to add an appropriate amount of steel slag or iron beans or lump stones to increase the FeO content in the slag, assist the melting of lime and dolomite, and improve the dephosphorization and desulfurization capacity of the slag. In addition, the gun position is controlled from high to low.
3. Improvement of slag making method. In order to ensure the dephosphorization and desulfurization effect of the slag, the slag containing TiO2 should be poured out to avoid affecting the removal of phosphorus and sulfur in the later stage of smelting, that is, double slag operation is adopted. Since titanium is oxidized before silicon, titanium is completely oxidized in the early stage of smelting. After titanium is completely oxidized, the slag containing TiO2 is removed and re-slag is made, which can avoid the problem that TiO2 increases the viscosity of the slag and reduces the utilization rate of white ash.
4. Selection of slag pouring timing. Studies have shown that in the blowing process of titanium-containing molten iron, the titanium-oxygen equilibrium constant increases with the increase of temperature. As the temperature increases, the oxidation ability of oxygen to titanium decreases. The conversion temperature of the selective oxidation of titanium in molten iron is 1340℃-1400℃. Therefore, in the converter smelting process, the early stage of blowing is a favorable stage for removing titanium from steel. For a 60-ton converter, the average pouring temperature is around 1370℃, which falls within the temperature range of 1340℃-1400℃. Therefore, the slag pouring timing is selected at the 1/4 moment of blowing, and the best time is to control the stability of the slag in the furnace for more than 30 seconds after foaming.
5. Operation optimization after slag pouring. After slag pouring, the basicity should be controlled at 2.8-3.2, and it should be adjusted appropriately according to the phosphorus content requirements of the steel grade. Low-phosphorus steel should be controlled according to the upper limit. The amount of dolomite added is controlled according to the MgO content of 10%-11% in the final slag, so as to meet the requirements of slag splashing and furnace protection.
6. The focus of the later smelting operation is slag reduction. Because the SiO2 content in the slag is low, an appropriate amount of iron-containing slag reduction agent should be added at the beginning of the secondary blowing to increase the FeO content in the slag, assist the melting of lime and dolomite, and improve the dephosphorization and desulfurization capacity of the slag, and the position should be controlled from high to low.
7. Improvement of heat balance calculation method. Titanium oxidizes and releases heat during the converter smelting process. When the titanium content in the molten iron is 0.10%-0.20%, the heat generation is large. Therefore, the heat increase of this part must be considered when calculating the heat balance to accurately control the final temperature. During on-site operation, titanium and silicon can be treated consistently in terms of the amount of heat released during the converter smelting process. The titanium and silicon contents in the molten iron should be comprehensively considered during heat balance calculations, and appropriate adjustments should be made to the loading system, i.e., the amount of scrap steel and coolant used should be adjusted while taking into account the effect of early slag discharge on the temperature, in order to accurately control the smelting endpoint temperature.