Ladle refining is a crucial step in steelmaking, and breathable bricks are the most critical functional components in this process. Their performance is essential for the smooth implementation of refining and ensuring steel quality and output. Damage to ladle permeable bricks mainly occurs in two ways: physical corrosion caused by melting and spalling, and chemical corrosion caused by slag and molten steel seeping into the breathable bricks. Currently, most permeable bricks in my country are still made of chromium corundum, but their performance cannot be significantly improved, and chromium also pollutes the environment. Therefore, corundum-spinel permeable bricks made primarily from fused alumina and spinel have been developed.

01 Experiment
The following raw materials were used: fused white corundum (w(Al₂O₃)>98.5%, w(Na₂O)<0.6%), spinel (w(Al₂O₃)>90%, w(MgO)>8%), magnesia (w(MgO)>99%), α-Al₂O₃ micro powder (w(Al₂O₃)>99%, Dv50=1.64μm), CA80 cement (Kaifeng Bianhe), silica fume (Norway 983), and zircon micro powder. Under the condition of unchanged particle size distribution, the content of some components in the matrix was varied. Strip samples of 160mm×40mm×40mm were vibrated and molded. After curing at room temperature for 24h and drying at 110℃ for 24h, the samples were fired at 1550℃ for 3h. The bulk density and apparent porosity of the samples were measured, and the slag resistance was tested using the static crucible method. The chemical composition (w) of the slag used in the experiment was: Al₂O₃ 45.01%, SiO₂ 14.56%, Fe₂O₃ 1.30%, CaO 21.55%, MgO 13.32%, FeO 2.66%, MFe 1.16%, S 0.03%, P 0.17%. Thermal shock stability was determined by subjecting strip specimens to a 1100℃ water-cooling cycle test.
02 Results and Discussion
2.1 Effect of MgO Content in the Matrix on Specimen Properties
Table 1 shows the effect of MgO content in the matrix on the specimen properties.
| Material | Corundum-Spinel | Chromium Corundum |
| Bulk density/g·cm−3 | 3.27 | 3.32 |
| Apparent porosity/% | 13 | 15 |
| Linear change rate/% | -0.4 | -0.1 |
| Flexural strength/MPa | 26.4 | 29.3 |
| Reheat linear change/% | 0.06 | -0.04 |
| Thermal shock resistance/cycles | 4.5 | 1.5 |
| Erosion index | 21 | 21 |
| Permeability index | 55 | 37 |
As shown in Table 1, with the increase of MgO content in the matrix, the bulk density of the sample decreases and the apparent porosity increases. The main reason is that MgO in the matrix reacts with fine corundum powder to form magnesium aluminum spinel, causing expansion; with the increase of MgO content, the linear shrinkage gradually decreases; when the MgO content is 5%, the amount of magnesium aluminum spinel (bound phase) in the sample increases, thus increasing the flexural strength at room temperature; when the MgO content in the matrix is in the range of 3% to 5%, the thermal shock stability and resistance to erosion by ladle refining slag of the sample do not change significantly.
2.2 Comparison of the properties of chrome corundum bricks and corundum-spinel bricks
The performance comparison of chrome corundum bricks and corundum-spinel bricks is shown in Table 2. It can be seen that there are some differences in the properties of the two types of bricks. Generally speaking, under the same particle size distribution, the bulk density of corundum-spinel bricks is lower than that of chrome corundum bricks. Table 2 also shows that the porosity of corundum-spinel bricks is lower than that of chrome corundum bricks. This is likely because the expansion of spinel during firing offsets the shrinkage of fine powder. Furthermore, the linear shrinkage rate of corundum-spinel bricks is greater than that of chrome corundum bricks, meaning that the volume stability of corundum-spinel bricks is inferior to that of chrome corundum bricks. This is mainly due to the formation of magnesium aluminum spinel during firing, a point that must be considered. Because the slots in the core of slotted permeable bricks are relatively narrow (generally around 200 μm), significant volume changes during firing will affect the size of the slots, ultimately impacting air permeability and leading to a decrease in the performance of the permeable bricks, or even complete blockage. The thermal shock stability of corundum-spinel bricks is better than that of chrome corundum bricks, possibly because spinel has better thermal shock stability than corundum.
| Material | Corundum-Spinel | Chromium Corundum |
| Bulk density/g·cm−3 | 3.27 | 3.32 |
| Apparent porosity/% | 13 | 15 |
| Linear change rate/% | -0.4 | -0.1 |
| Flexural strength/MPa | 26.4 | 29.3 |
| Reheat linear change/% | 0.06 | -0.04 |
| Thermal shock resistance/cycles | 4.5 | 1.5 |
| Erosion index | 21 | 21 |
| Permeability index | 55 | 37 |
03 Industrial Trial
3.1 Trial Production Process
The breathable bricks core and base brick were respectively made of corundum-spinel and brown corundum-spinel. The corundum-spinel material used for the brick core had good molding performance, slow venting, and a longer vibration time than chromium corundum. The flow value was 110-120mm (jump table method), and it did not delaminate. After demolding, the brick core felt strong, and the edges and corners remained intact. After drying and curing, the brick core was fired at 1580℃, and the base brick was baked at 450℃ in a kiln after drying and curing.
3.2 Application
One set was composed of high-purity corundum-spinel as the brick core and chromium corundum as the base brick, and another set was composed of chromium corundum as the brick core and brown corundum-spinel as the base brick. These sets were used on the ladles of the No. 2 Steelmaking Plant of Wuhan Iron and Steel Company. The ladles of the No. 2 Steelmaking Plant of Wuhan Iron and Steel Company are not dedicated ladles, and the steel grades smelted in a single ladle vary greatly, which has a significant impact on the use of breathable bricks. Therefore, the trial bricks were divided into two groups and compared with chrome corundum breathable bricks. The average corrosion rate of the corundum-spinel base brick was the lowest, and its erosion resistance was significantly improved compared with the original base brick. The bottom blowing rate of the core of the permeable brick exceeded 98%.
04 Conclusions
(1) The MgO content in the matrix has a significant impact on the performance of corundum-spinel permeable bricks (core and base brick).
(2) The thermal shock stability of the developed corundum-spinel brick is worse than that of traditional chrome corundum bricks, but its volume stability is not as good as that of chrome corundum bricks. Strict control is required in industrial production.
(3) Industrial tests show that the performance of corundum-spinel breathable brick is no less than that of traditional chrome corundum bricks.